A method for reducing the width of the softening zone of high-strength pearlite rail joints
By controlling various parameters of the welding process, the softening zone width of the high-strength pearlite rail joints is reduced, and the problem of poor performance of rail welded joints in heavy-duty railway lines is solved, and the joint performance optimization and standard compliance are achieved.
Patent Information
- Application Number
- CN202211368320.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-03
AI Technical Summary
The prior art is difficult to effectively reduce the softening zone width of high-strength pearlite rail joints, resulting in poor performance of rail welded joints of heavy-duty railway lines and prone to fatigue or brittle fracture.
By controlling the various parameters of the welding process, including pre-flash, flash, accelerated burning, top forging and forging, adjusting high-voltage time, voltage, flash speed, top forging and forging time, we can reduce the softening area of the rail joints by adjusting the high-voltage time, voltage, flash speed, top forging and forging time, to reduce the softening area of the rail joints. width.
The softening zone width of the high-strength pearlite rail joint is successfully controlled within the range of 5mm to 10mm, which is far beyond the technical indicator requirements specified in the standard. At the same time, the performance of the welded joint is optimized and meets the use standards of heavy-duty railways.
Smart Images

Figure CN115870595B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rail welding, and in particular to a method for reducing the width of a softening zone of a high-strength pearlite rail joint. Background Art
[0002] A large number of studies have shown that rail weld joint damage accounts for a large proportion of the total damage of heavy-load lines at home and abroad, and is the focus of attention of railway lines. During the service of rail weld joints, the bonding strength of the rail joint determines whether the rail joint is prone to fatigue or brittle fracture, and the longitudinal section hardness of the rail joint determines the smoothness of different micro-areas of the joint.
[0003] The softening zone of the rail flash weld joint refers to the area where the hardness of the weld joint is significantly lower than that of the parent material, and the hardness of the rail joint softens. Unlike the austenitized area of the joint, which has a lower hardness than the parent material, the metal in the softening zone does not undergo austenite transformation during the heating process, and its temperature range is usually in the annealing range of metal heat treatment, so the softening zone is sometimes called the annealing zone. Because the rail material is usually a granular pearlite structure after annealing, the softening zone is also called the spheroidizing annealing zone. In general, the tensile and impact properties of the joint softening zone are poor, which is the weak link of the rail joint. Because rail welding mainly heats the end of the rail locally, there is always a transition zone between the heated part and the unheated parent material. The area with lower hardness in the transition zone is the softening zone. The softening zone is an area that always exists in the rail weld joint and cannot be completely eliminated. Under the same welding and post-weld treatment methods, the softening zones of rail joints with different chemical compositions and delivery states are different. The Australian standard AS stipulates that the softening zone width of rails of different materials ranges from 20mm to 40mm. Generally speaking, the narrower the softening zone, the better the service performance of the joint. Therefore, reducing the softening zone width of the rail joint is a favorable way to improve the joint quality.
[0004] However, compared with ordinary lines or high-speed railway lines, the main feature of heavy-duty railway lines is the heavy axle weight. Current research shows that axle weight is the factor that has the greatest impact on the on-road service performance of rails. The wear of rail parent materials and joints, rolling contact fatigue damage, impact dynamic loads, and brittle fractures are all more serious with the increase of axle weight. In order to improve the wear performance that is most needed for heavy-duty line rails, the strength and hardness of heavy-duty rails are relatively high. The higher the strength and hardness of the rails, the worse the welding performance of the rails. The welded joints are the weak link in the railway line. The optimization of the performance of heavy-duty rail welded joints is still the research focus of existing technology centers.
[0005] Therefore, there is a need in the prior art for an improved method of reducing the softening zone of high-strength pearlite rail joints. Summary of the invention
[0006] In view of this, the purpose of the embodiment of the present invention is to propose a method for reducing the width of the softening zone of a high-strength pearlite rail joint, which effectively reduces the width of the softening zone by controlling various parameters of the welding process, far exceeding the technical index requirements specified in the standard.
[0007] Based on the above purpose, an embodiment of the present invention provides a method for reducing the width of the softening zone of a high-strength pearlite rail joint, the method comprising the following steps:
[0008] The welding of rail joints includes five stages: pre-flash, flash, accelerated burning, upsetting and forging. The pre-flash and flash stages are used to prepare the rail surface to be welded by flash blasting. The accelerated burning stage controls the accelerated burning voltage and flash acceleration speed. The upsetting stage controls the upsetting amount. The forging stage controls the rail consumption and forging time to reduce the width of the softening zone.
[0009] By weight percentage, the high-strength pearlite rail includes 0.72% to 0.86% carbon, 0.10% to 1.00% silicon, 0.60% to 1.30% manganese, no more than 0.020% phosphorus, no more than 0.020% sulfur, no more than 0.3% chromium, and no more than 0.01% vanadium.
[0010] In some embodiments, the high voltage time of the pre-flash stage is 45s to 65s, the high voltage is 370V to 440V, the pre-flash distance is 2mm to 10mm, and the flash speed is 0.1mm / s to 0.6mm / s.
[0011] In some embodiments, the low voltage time in the flashing stage is 80s to 140s, the low voltage is 320V to 390V, and the flashing speed is 0.1mm / s to 0.6mm / s.
[0012] In some embodiments, the accelerated burning voltage in the accelerated burning stage is 380V to 450V, and the flash acceleration speed is 0.5mm / s to 2.0mm / s.
[0013] In some embodiments, the upsetting amount in the upsetting stage is 5.0 mm to 18.0 mm.
[0014] In some embodiments, the rail consumption in the forging stage is 2.0 mm to 4.0 mm, and the forging time is 1.5 s to 3.0 s.
[0015] In some embodiments, the rail joints are flash welded using moving welding.
[0016] Another aspect of the present invention provides a high-strength pearlite rail joint processed by the above method, wherein the width of the softening zone of the high-strength pearlite rail joint is 5 mm to 10 mm.
[0017] The present invention has at least the following beneficial technical effects:
[0018] The method of the present invention divides the welding process into five main stages, namely, pre-flash, flash, accelerated burning, top forging and forging, and effectively reduces the softening zone width of the high-strength pearlite rail joint by controlling various parameters of the welding process, and optimizes the performance of the heavy-load rail welding joint. The softening zone width of the high-strength pearlite rail joint for heavy-load railway welded by the method is at a good level of 5 mm to 10 mm, and the softening zone widths on both sides of the fusion line are equivalent, and the difference between the maximum value and the minimum value is 1 mm to 4 mm, which far exceeds the technical index requirements specified in the standard, and the other properties of the joint also meet the standard requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A schematic diagram of an embodiment of the softening zone of a high-strength pearlite rail flash weld joint provided by the present invention. DETAILED DESCRIPTION
[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0022] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0023] Aiming at the problem that the width of the softening zone of the continuous flash welded joint of high-strength pearlite rail for heavy-duty railway is too wide to meet the standard requirements, the present invention provides a method for reducing the width of the softening zone of the high-strength pearlite rail joint, such as Figure 1 The figure shows a schematic diagram of the softening zone of the rail flash weld joint provided by the present invention. The method of the present invention comprises the following steps:
[0024] The welding of rail joints includes five stages: pre-flash, flash, accelerated burning, upsetting and forging. The pre-flash and flash stages are used to prepare the rail surface to be welded by flash blasting. The accelerated burning stage controls the accelerated burning voltage and flash acceleration speed. The upsetting stage controls the upsetting amount. The forging stage controls the rail consumption and forging time to reduce the width of the softening zone.
[0025] By weight percentage, the high-strength pearlite rail includes 0.72% to 0.86% carbon, 0.10% to 1.00% silicon, 0.60% to 1.30% manganese, no more than 0.020% phosphorus and sulfur, no more than 0.3% chromium, and no more than 0.01% vanadium.
[0026] Furthermore, the minimum tensile strength of the rail is 1080 MPa and the minimum hardness of the rail head is 310 HB.
[0027] In the above-mentioned continuous flash welding, the flash process is mainly realized by pre-flash, flash, and accelerated burning, and the flash process is smooth, continuous and uninterrupted. In order to achieve the purpose of reducing the width of the softening zone of the high-strength pearlite rail joint, it is necessary to strictly control the heat input, heat conduction time and high-temperature rail consumption at each stage of the welding process.
[0028] The main function of the above-mentioned pre-flash stage is to make the cross section of the rail to be welded flat and clean through flash blasting, providing relatively uniform and flat favorable conditions and basic heat for subsequent flashing. In order to achieve the purpose of controlling heat, heat conduction time and high-temperature rail consumption, it is mainly necessary to control the high-voltage time, high voltage, pre-flash distance and flash speed in this stage. In some embodiments, the high-voltage time of the pre-flash stage is 45s to 65s, the high voltage is 370V to 440V, the pre-flash distance is 2mm to 10mm, and the flash speed is 0.1mm / s to 0.6mm / s.
[0029] The main function of the above-mentioned flash stage is to make the cross section of the rail to be welded flat and clean through flash blasting, providing relatively uniform and flat favorable conditions and basic heat for subsequent flashing. In order to achieve the purpose of controlling heat and heat conduction time, it is mainly necessary to control the low-voltage time, low voltage and flash speed of this stage. In some embodiments, the low-voltage time of the flash stage is 80s to 140s, the low voltage is 320V to 390V, and the flash speed is 0.1mm / s to 0.6mm / s.
[0030] The main function of the above-mentioned accelerated burning stage is to form a protective atmosphere in the entire welding area to prevent end face oxidation, and finally form a suitable temperature field distribution to provide conditions for top forging. In order to achieve the purpose of controlling the amount of heat and heat conduction time, it is mainly necessary to control the accelerated burning voltage and flash acceleration speed in this stage. In some embodiments, the accelerated burning voltage of the accelerated burning stage is 380V to 450V, and the acceleration speed is 0.5mm / s to 2.0mm / s.
[0031] The main function of the above-mentioned upset forging stage is to make the steel rails to be welded in a high-temperature plastic state produce atomic bonding. In order to achieve the purpose of controlling the consumption of the steel rails, it is mainly necessary to control the upset amount of this stage. In some embodiments, the upset amount of the upset forging stage is 5.0 mm to 18.0 mm.
[0032] The main function of the forging stage is to continuously apply load to the rail joint during the metal crystallization process of the joint after the rail top forging. In order to achieve the purpose of controlling the rail consumption to further reduce the width of the softening zone of the high-strength pearlite rail joint, it is mainly necessary to control the rail consumption and forging time in this stage. In some embodiments, the rail consumption in the forging stage is 2.0 mm to 4.0 mm, and the forging time is 1.5 s to 3.0 s.
[0033] On the other hand, the present invention also provides a high-strength pearlite rail joint processed by the above method, wherein the width of the softening zone of the rail joint is at a good level of 5 mm to 10 mm, and the width of the softening zones on both sides of the fusion line is equivalent, and the difference between the maximum and minimum values is 1 mm to 4 mm, far exceeding the technical index requirements specified in the standard.
[0034] The present invention will be further explained below based on specific embodiments.
[0035] Example 1
[0036] In this embodiment, the mass fraction of carbon in the test rail material is 0.73%, the mass fraction of silicon is 0.81%, and the mass fraction of manganese is 1.12%. The tensile strength of the rail is 1180MPa-1200MPa, and the rail head hardness is 310HB-320HB. The high voltage time of the pre-flash stage of continuous flash welding is 45s, the high voltage is 370V, the pre-flash distance is 10mm, and the flash speed is 0.6mm / s; the low voltage time of the flash stage is 80s, the low voltage is 320V, and the flash speed is 0.6mm / s; the accelerated burning voltage of the accelerated burning stage is 380V, and the acceleration speed is 2.0mm / s; the upsetting amount of the upsetting stage is 18.0mm; the rail consumption in the forging stage is 4.0mm, and the forging time is 3.0s. After inspection, it was found that the widths of the softening zones on the left and right sides of the rail joint in this embodiment were 6mm and 7mm respectively, and the difference between the maximum and minimum values was 1mm, which far exceeded the technical index requirements specified in the standard, and the other performances of the joint also met the standard requirements.
[0037] Example 2
[0038] In this embodiment, the mass fraction of carbon in the test rail material is 0.73%, the mass fraction of silicon is 0.81%, and the mass fraction of manganese is 1.12%. The tensile strength of the rail is 1180MPa-1200MPa, and the rail head hardness is 310HB-320HB. The high voltage time of the pre-flash stage of continuous flash welding is 65s, the high voltage is 440V, the pre-flash distance is 2mm, and the flash speed is 0.1mm / s; the low voltage time of the flash stage is 140s, the low voltage is 390V, and the flash speed is 0.1mm / s; the accelerated burning voltage of the accelerated burning stage is 450V, and the acceleration speed is 0.5mm / s; the upsetting amount of the upsetting stage is 5.0mm; the rail consumption in the forging stage is 2.0mm, and the forging time is 1.5s. After inspection, it was found that the widths of the softening zones on the left and right sides of the rail joint in this embodiment were 9 mm and 5 mm respectively, and the difference between the maximum and minimum values was 4 mm, which far exceeded the technical index requirements specified in the standard, and the other performances of the joint also met the standard requirements.
[0039] Example 3
[0040] In this embodiment, the mass fraction of carbon in the test rail material is 0.86%, the mass fraction of silicon is 0.58%, and the mass fraction of manganese is 0.81%. The tensile strength of the rail is 1280MPa-1420MPa, and the rail head hardness is 370HB-420HB. The high voltage time of the pre-flash stage of continuous flash welding is 45s, the high voltage is 370V, the pre-flash distance is 10mm, and the flash speed is 0.6mm / s; the low voltage time of the flash stage is 80s, the low voltage is 320V, and the flash speed is 0.6mm / s; the accelerated burning voltage of the accelerated burning stage is 380V, and the acceleration speed is 2.0mm / s; the upsetting amount of the upsetting stage is 18.0mm; the rail consumption in the forging stage is 4.0mm, and the forging time is 3.0. After inspection, it was found that the widths of the softening zones on the left and right sides of the rail joint in this embodiment were 5mm and 7mm respectively, and the difference between the maximum and minimum values was 2mm, which far exceeded the technical index requirements specified in the standard, and the other performances of the joint also met the standard requirements.
[0041] Example 4
[0042] In the present embodiment, the mass fraction of carbon in the test rail material is 0.86%, the mass fraction of silicon is 0.58%, and the mass fraction of manganese is 0.81%. The tensile strength of the rail is 1280MPa-1420MPa, and the rail head hardness is 400HB-420HB. The high voltage time of the pre-flash stage of continuous flash welding is 65s, the high voltage is 440V, the pre-flash distance is 2mm, and the flash speed is 0.1mm / s; the low voltage time of the flash stage is 140s, the low voltage is 390V, and the flash speed is 0.1mm / s; the accelerated burning voltage of the accelerated burning stage is 450V, and the acceleration speed is 0.5mm / s; the upsetting amount of the upsetting stage is 5.0mm; the rail consumption in the forging stage is 2.0mm, and the forging time is 1.5s. After inspection, it was found that the widths of the softening zones on the left and right sides of the rail joint in this embodiment were 9 mm and 6 mm respectively, and the difference between the maximum and minimum values was 3 mm, which far exceeded the technical index requirements specified in the standard, and the other performances of the joint also met the standard requirements.
[0043] Example 5
[0044] In this embodiment, the mass fraction of carbon in the test rail material is 0.82%, the mass fraction of silicon is 0.70%, and the mass fraction of manganese is 0.92%. The tensile strength of the rail is 1180MPa-1300MPa, and the rail head hardness is 350HB-410HB. The high voltage time of the pre-flash stage of continuous flash welding is 50s, the high voltage is 4050V, the pre-flash distance is 5mm, and the flash speed is 0.3mm / s; the low voltage time of the flash stage is 110s, the low voltage is 385V, and the flash speed is 0.5mm / s; the accelerated burning voltage of the accelerated burning stage is 420V, and the acceleration speed is 1.2mm / s; the upsetting amount of the upsetting stage is 11.0mm; the rail consumption in the forging stage is 2.6mm, and the forging time is 2.1s. After inspection, it was found that the widths of the softening zones on the left and right sides of the rail joint in this embodiment were 9 mm and 7 mm respectively, and the difference between the maximum and minimum values was 2 mm, which far exceeded the technical index requirements specified in the standard, and the other performances of the joint also met the standard requirements.
[0045] Comparative Example 1
[0046] The mass fraction of carbon in the test rail material in this comparative example is 0.73%, the mass fraction of silicon is 0.81%, and the mass fraction of manganese is 1.12%. The tensile strength of the rail is 1180MPa~1200MPa, and the rail head hardness is 310HB~320HB. The high voltage time of the pre-flash stage of continuous flash welding is 40s, the high voltage is 360V, the pre-flash distance is 11mm, and the flash speed is 0.7mm / s; the low voltage time of the flash stage is 70s, the low voltage is 310V, and the flash speed is 0.8mm / s; the accelerated burning voltage of the accelerated burning stage is 375V, and the acceleration speed is 2.3mm / s; the upsetting amount of the upsetting stage is 19.0mm; the rail consumption in the forging stage is 5.2mm, and the forging time is 3.4s. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 4mm and 5mm respectively, the difference in the widths of the softening zones on the left and right sides of the fusion line is 1mm, and during the static bending test, when the static bending load reaches 800kN, the joint breaks, which does not meet the standard requirements. The main difference between this comparative example and Examples 1 and 2 lies in the welding method. The high-voltage time and low-voltage time used in the comparative example are lower than those in the specific embodiment of the present invention, the continuous flash process is short, and the welding heat input is small; the voltage value used is lower than the specific embodiment of the present invention, the continuous flash process is not violent, and the welding heat input is small; the flash speed of each stage is higher than that of the specific embodiment of the present invention, the high-temperature metal is consumed quickly, the heat loss is fast, and the welding heat input is small; the top amount, forging amount and time are higher than those in the specific embodiment of the present invention, the rail consumes more high temperature, the heat loss is large, and a "cold joint" is formed. Although the softening zone is narrow, the other properties of the joint drop sharply. Under the condition of the same rail material, the method of this comparative example cannot achieve the expected effect.
[0047] Comparative Example 2
[0048] The mass fraction of carbon in the test rail material in this comparative example is 0.73%, the mass fraction of silicon is 0.81%, and the mass fraction of manganese is 1.12%. The tensile strength of the rail is 1180MPa~1200MPa, and the rail head hardness is 310HB~320HB. The high voltage time of the pre-flash stage of continuous flash welding is 69s, the high voltage is 450V, the pre-flash distance is 2mm, and the flash speed is 0.1mm / s; the low voltage time of the flash stage is 152s, the low voltage is 400V, and the flash speed is 0.1mm / s; the accelerated burning voltage of the accelerated burning stage is 420V, and the acceleration speed is 0.4mm / s; the upsetting amount of the upsetting stage is 4.0mm; the rail consumption in the forging stage is 0.5mm, and the forging time is 1.0s. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 22mm and 23mm respectively, and the difference in the widths of the softening zones on the left and right sides of the fusion line is 1mm, which does not meet the standard requirements. The main difference between this comparative example and Examples 1 and 2 lies in the welding method. The comparative example uses higher high-pressure time and low-pressure time than the specific embodiment of the present invention, and the continuous flash process is long, and the welding heat input is large; the voltage value used is higher than the specific embodiment of the present invention, and the continuous flash process is violent, and the welding heat input is large; the flash speed of each stage is lower than the specific embodiment of the present invention, and the high-temperature metal consumption is small, the heat loss is small, and the welding heat input is large; the top amount, forging amount and time are lower than the specific embodiment of the present invention, the rail high-temperature consumption is small, the heat loss is small, and the width of the joint softening zone is too wide. When the rail material is the same, the method of this comparative example cannot achieve the expected effect.
[0049] Comparative Example 3
[0050] The mass fraction of carbon in the test rail material in this comparative example is 0.86%, the mass fraction of silicon is 0.58%, and the mass fraction of manganese is 0.81%. The tensile strength of the rail is 1280MPa~1420MPa, and the rail head hardness is 370HB~420HB. The high voltage time of the pre-flash stage of continuous flash welding is 40s, the high voltage is 360V, the pre-flash distance is 11mm, and the flash speed is 0.7mm / s; the low voltage time of the flash stage is 70s, the low voltage is 310V, and the flash speed is 0.8mm / s; the accelerated burning voltage of the accelerated burning stage is 375V, and the acceleration speed is 2.3mm / s; the upsetting amount of the upsetting stage is 19.0mm; the rail consumption in the forging stage is 5.2mm, and the forging time is 3.4s. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 4mm and 5mm respectively, the difference in the widths of the softening zones on the left and right sides of the fusion line is 1mm, and during the static bending test, when the static bending load reaches 800kN, the joint breaks, which does not meet the standard requirements. The main difference between this comparative example and Examples 3 and 4 lies in the welding method. The high-pressure time and low-pressure time used in the comparative example are lower than those in the specific embodiment of the present invention, the continuous flash process is short, and the welding heat input is small; the voltage value used is lower than the specific embodiment of the present invention, the continuous flash process is not violent, and the welding heat input is small; the flash speed of each stage is higher than that of the specific embodiment of the present invention, the high-temperature metal is consumed quickly, the heat loss is fast, and the welding heat input is small; the top amount, forging amount and time are higher than those in the specific embodiment of the present invention, the rail consumes more high temperature, the heat loss is large, and a "cold joint" is formed. Although the softening zone is narrow, the other properties of the joint drop sharply. Under the condition of the same rail material, the method of this comparative example cannot achieve the expected effect.
[0051] Comparative Example 4
[0052] The mass fraction of carbon in the test rail material in this comparative example is 0.86%, the mass fraction of silicon is 0.58%, and the mass fraction of manganese is 0.81%. The tensile strength of the rail is 1280MPa~1420MPa, and the rail head hardness is 370HB~420HB. The high voltage time of the pre-flash stage of continuous flash welding is 80s, the high voltage is 420V, the pre-flash distance is 2mm, and the flash speed is 0.1mm / s; the low voltage time of the flash stage is 170s, the low voltage is 400V, and the flash speed is 0.1mm / s; the accelerated burning voltage of the accelerated burning stage is 420V, and the acceleration speed is 2.5mm / s; the upsetting amount of the upsetting stage is 3.0mm; the rail consumption in the forging stage is 2.0mm, and the forging time is 1.0. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 25mm and 26mm respectively, and the difference in the widths of the softening zones on the left and right sides of the fusion line is 1mm, which does not meet the standard requirements. At the same time, in the static bending test, when the static bending load reaches 1500kN, the joint breaks, and the maximum deflection value is 8.4mm, which does not meet the standard requirements. The main difference between this comparative example and Example 3 and Example 4 lies in the welding method. The comparative example adopts a high-pressure time and low-pressure time higher than the specific embodiment of the present invention, the continuous flash process is long, and the welding heat input is large; the voltage value higher than the specific embodiment of the present invention is adopted, the continuous flash process is violent, and the welding heat input is large; the flash speed of each stage is lower than the specific embodiment of the present invention, the high-temperature metal consumption is small, the heat loss is small, and the welding heat input is large; the top amount and forging amount and time lower than the specific embodiment of the present invention are adopted, the rail high temperature consumption is small, the heat loss is small, and the width of the joint softening zone is too wide. At the same time, when the welding heat input is too large and the top forging amount is too small, the rail bonding strength is reduced, and the static bending performance drops sharply. When the rail material is the same, the expected effect cannot be achieved by using this comparative method.
[0053] Comparative Example 5
[0054] The mass fraction of carbon in the test rail material in this comparative example is 0.82%, the mass fraction of silicon is 0.70%, and the mass fraction of manganese is 0.92%. The tensile strength of the rail is 1180MPa~1300MPa, and the rail head hardness is 350HB~410HB. The high voltage time of the pre-flash stage of continuous flash welding is 40s, the high voltage is 360V, the pre-flash distance is 11mm, and the flash speed is 0.7mm / s; the low voltage time of the flash stage is 70s, the low voltage is 310V, and the flash speed is 0.8mm / s; the accelerated burning voltage of the accelerated burning stage is 375V, and the acceleration speed is 2.3mm / s; the upsetting amount of the upsetting stage is 20.0mm; the rail consumption in the forging stage is 5.2mm, and the forging time is 3.4s. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 3mm and 5mm respectively, and the difference in the widths of the softening zones on the left and right sides of the fusion line is 2mm. In addition, during the static bending test, when the static bending load reaches 1000kN, the joint breaks, and the maximum deflection value is 7.6mm, which does not meet the standard requirements, and abnormal martensitic structure is detected at the standard inspection position of the joint, which does not meet the standard requirements. The main difference between this comparative example and Example 5 lies in the welding method. The comparative example adopts a high-pressure time and low-pressure time lower than the specific embodiment of the present invention, the continuous flash process is short, and the welding heat input is small; the voltage value lower than the specific embodiment of the present invention is adopted, the continuous flash process is not violent, and the welding heat input is small; the flash speed of each stage is higher than the specific embodiment of the present invention, the high-temperature metal is consumed quickly, the heat loss is fast, and the welding heat input is small; the top amount, forging amount and time higher than the specific embodiment of the present invention are adopted, the rail high temperature consumption is large, the heat loss is large, and a "cold joint" is formed. Although the softening zone is narrow, the other properties of the joint are sharply reduced. At the same time, due to the small heat input of the joint, the cooling rate during the cooling process is large, and the martensitic phase transformation is easy to occur in the local area. Under the condition of the same rail material, the comparative method cannot achieve the expected effect.
[0055] Comparative Example 6
[0056] The mass fraction of carbon in the test rail material in this comparative example is 0.82%, the mass fraction of silicon is 0.70%, and the mass fraction of manganese is 0.92%. The tensile strength of the rail is 1180MPa~1300MPa, and the rail head hardness is 350HB~410HB. The high voltage time of the pre-flash stage of continuous flash welding is 85s, the high voltage is 415V, the pre-flash distance is 2mm, and the flash speed is 0.1mm / s; the low voltage time of the flash stage is 172s, the low voltage is 410V, and the flash speed is 0.1mm / s; the accelerated burning voltage of the accelerated burning stage is 425V, and the acceleration speed is 2.5mm / s; the upsetting amount of the upsetting stage is 3.0mm; the rail consumption in the forging stage is 2.0mm, and the forging time is 1.0. After inspection, the widths of the softening zones on the left and right sides of the rail joint in this comparative example are 24mm and 25mm respectively, and the difference in the width of the softening zones on the left and right sides of the fusion line is 1mm, which does not meet the standard requirements. At the same time, in the static bending test, when the static bending load reaches 1600kN, the joint breaks, and the maximum deflection value is 9.3mm, which does not meet the standard requirements. The main difference between this comparative example and Example 5 lies in the welding method. The comparative example adopts a higher high-pressure time and low-pressure time than the specific embodiment of the present invention, the continuous flash process is long, and the welding heat input is large; the voltage value is higher than the specific embodiment of the present invention, the continuous flash process is violent, and the welding heat input is large; the flash speed of each stage is lower than the specific embodiment of the present invention, the high-temperature metal consumption is small, the heat loss is small, and the welding heat input is large; the top amount and forging amount and time are lower than the specific embodiment of the present invention, the rail high temperature consumption is small, the heat loss is small, and the width of the joint softening zone is too wide. At the same time, when the welding heat input is too large and the top forging amount is too small, the rail bonding strength is reduced, and the static bending performance drops sharply. Under the condition of the same rail material, the method of this comparative example cannot achieve the expected effect.
[0057] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0058] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.
[0059] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0060] A person skilled in the art will understand that all or part of the steps to implement the above embodiments may be accomplished by hardware or by instructing related hardware through a program, and the program may be stored in a computer-readable storage medium, and the above-mentioned storage medium may be a read-only memory, a disk or an optical disk, etc.
[0061] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for reducing the width of the softening zone of a high-strength pearlite rail joint, characterized in that: The rail joint welding process includes five stages: pre-flash, flash, accelerated burn-in, upset and forging. The pre-flash and flash stages are used to prepare the rail surface to be welded by flash blasting. The accelerated burn-in stage controls the accelerated burn-in voltage and the flash acceleration speed. The upset stage controls the upset amount. The forging stage controls the rail consumption and forging time to reduce the width of the softening zone. High-strength pearlite rails contain, by weight percentage, 0.72% to 0.86% carbon, 0.10% to 1.00% silicon, 0.60% to 1.30% manganese, not more than 0.020% phosphorus, not more than 0.020% sulfur, not more than 0.3% chromium, and not more than 0.01% vanadium; The high-voltage time of the pre-flash stage is 45s to 65s, the high voltage is 370V to 440V, the pre-flash distance is 2mm to 10mm, and the flash speed is 0.1mm / s to 0.6mm / s; The low voltage time of the flashing stage is 80s to 140s, the low voltage is 320V to 390V, and the flashing speed is 0.1mm / s to 0.6mm / s; The accelerated burning voltage in the accelerated burning stage is 380V to 450V, and the flash acceleration speed is 0.5mm / s to 2.0mm / s; The upset amount in the upset stage is 5.0 mm to 18.0 mm; The rail consumption in the forging stage is 2.0 mm to 4.0 mm, and the forging time is 1.5 s to 3.0 s.
2. The method for reducing the width of the softening zone of a high-strength pearlite rail joint according to claim 1, characterized in that: The rail joints are welded using mobile flash welding.
3. A high-strength pearlite rail joint processed by the method according to any one of the above claims, characterized in that: The width of the softening zone of the high-strength pearlite rail joint is 5mm to 10mm.