A high-strength oxide nanofiber porous thermal protection material and preparation method thereof

Through the high-strength composite of nano-scale oxide fibers and micro-scale oxide fibers and the impregnation treatment of nanoparticle precursors, the problem of loose structure and low strength of oxide nano-fiber thermal protection materials is solved, and high strength, high temperature resistance and The improvement of thermal insulation performance is suitable for the new generation of thermal protection materials.

CN115871289BActive Publication Date: 2024-11-22AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310019183.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-06
Publication Date
2024-11-22
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

The existing oxide nanofiber thermal protection materials have loose structure and low strength, which cannot meet the usage requirements.

Method used

High-strength composite of nano-scale oxide fibers and micro-scale oxide fibers is adopted to form an interpenetrating network structure through high-frequency needle puncture, and vacuum impregnation and high-temperature heat treatment with nanoparticle precursors are prepared to produce porous high-strength oxide nanofibers. Thermal protection material.

Benefits of technology

The material has excellent high temperature resistance, heat insulation and strength and toughness, and can meet the needs of heat insulation, heat resistance and load bearing at the same time, improving mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115871289B_ABST
    Figure CN115871289B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-strength oxide nanofiber porous thermal protection material, comprising a nano-scale oxide fiber layer and a micron-scale oxide fiber layer, wherein the nano-scale oxide fiber layer is laid on the surface of the micron-scale oxide fiber layer to form an interpenetrating network structure, and the nano-scale oxide fiber layer and the micron-scale oxide fiber layer both contain nanoparticles inside. The present invention also relates to a method for preparing a high-strength oxide nanofiber porous thermal protection material. The purpose of the high-strength oxide nanofiber porous thermal protection material and the preparation method thereof is to solve the problem of loose structure and low strength of the oxide nanofiber thermal protection material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermal protection material preparation technology, specifically to a high-strength oxide nanofiber porous thermal protection material and its preparation method. Background Technology

[0002] With the significant increase in aircraft speed, various structures face severe aerodynamic heating challenges, making "heat" and "force" crucial for structural design and material application. Traditional thermal protection materials mainly consist of rigid ceramic fiber heat-resistant tiles and flexible thermal insulation felts, which, while meeting the requirements of heat resistance and lightweight, offer poor thermal insulation performance. Therefore, aerogel materials have attracted widespread attention due to their excellent thermal insulation properties and ultra-low density. Currently, the most widespread application of aerogels remains in thermal insulation, but due to their weak skeletal structure, high brittleness, and inability to withstand loads, they need to be combined with other load-bearing structures. However, the thermal bridging effect within the structure can lead to a decrease in the overall thermal insulation performance. Oxide nanofibers possess a nanoscale skeletal structure with high structural strength and good toughness. Nanoporous materials composed of nanoscale oxide fibers can achieve high temperature resistance, low thermal conductivity, and good toughness, showing broad application prospects in the field of thermal protection technology.

[0003] Patent CN113663611A discloses a high-temperature resistant composite nanofiber aerogel material and its preparation method. First, tetraethyl orthosilicate, phosphoric acid, and water are mixed and stirred. Silicon carbide nanoparticles are then added and stirred continuously. After ultrasonic treatment, a composite hydrolysate is obtained. A polyvinyl alcohol aqueous solution and the composite hydrolysate are mixed evenly with water and stirred. Then, the precursor solution is electrospun to obtain a hybrid nanofiber membrane. The heat-treated hybrid nanofiber membrane, tetraethyl orthosilicate, boric acid, and aluminum chloride are added to water and stirred at high speed to obtain a homogeneous dispersion. This dispersion is then subjected to freezing, freeze-drying, composite polysilicon carbide, curing, and high-temperature pyrolysis processes to obtain the high-temperature resistant composite nanofiber aerogel material. The obtained material exhibits high elasticity, excellent radiation resistance, temperature resistance, and high-temperature insulation properties. However, the nanofiber aerogel material prepared by this method has a loose structure and low strength, which cannot meet the application requirements. Patent CN202210213909.X discloses an ultra-low thermal conductivity nanofiber aerogel composite material and its preparation method. The material is composed of nanofiber aerogel and oxide aerogel. The three-dimensional nanofiber aerogel prepared by freeze-drying technology is used as the reinforcement and combined with oxide aerogel to obtain a double network structure of layered fiber support framework and nanoporous aerogel composite. It has good thermal insulation performance, but the bonding force between nanoparticles and nanofibers is weak and the material is easy to pulverize.

[0004] Therefore, the inventors have provided a high-strength oxide nanofiber porous thermal protection material and its preparation method. Summary of the Invention

[0005] (1) Technical problems to be solved

[0006] This invention provides a high-strength oxide nanofiber porous thermal protection material and its preparation method, solving the technical problems of loose structure and low strength of oxide nanofiber thermal protection materials.

[0007] (2) Technical solution

[0008] This invention provides a high-strength oxide nanofiber porous thermal protection material, comprising a nanoscale oxide fiber layer and a micrometer-scale oxide fiber layer. The nanoscale oxide fiber layer is laid flat on the surface of the micrometer-scale oxide fiber layer and forms an interpenetrating network structure. Both the nanoscale oxide fiber layer and the micrometer-scale oxide fiber layer contain nanoparticles.

[0009] Furthermore, the fibers in the nanoscale oxide fiber layer are one or more of mullite nanofibers, SiO2 nanofibers, high-silica nanofibers, and carbon nanofibers.

[0010] Furthermore, the fibers in the micron-scale oxide fiber layer are one or more of mullite fibers, alumina fibers, quartz fibers, high-silica fibers, aluminum silicate fibers, and glass fibers.

[0011] Furthermore, the thickness of the nanoscale oxide fiber layer is 2–10 mm.

[0012] Furthermore, the thickness of the micron-sized oxide fiber layer is 3–20 mm.

[0013] This invention also provides a method for preparing a high-strength oxide nanofiber porous thermal protection material, comprising the following steps:

[0014] Step 1: The nanoscale oxide fiber is laid flat on the surface of the micron-scale oxide fiber, and the two materials are combined by high-frequency needle punching to form an interpenetrating network structure.

[0015] Step 2: Repeat Step 1 until the thickness of the upper nanofiber reaches the required thickness of the material, and obtain the interpenetrating network structure fiber preform.

[0016] Step 3: Prepare nanoparticle precursors;

[0017] Step 4: Place the interpenetrating network structure fiber preform into a vacuum impregnation mold and evacuate the vacuum.

[0018] Step 5: Pressurize the nanoparticle precursor into a vacuum impregnation mold in which the interpenetrating network structure fiber preform is placed, so that it is fully impregnated with the interpenetrating network structure fiber preform, and continue to evacuate the vacuum until the nanoparticle precursor is solidified to obtain a composite material.

[0019] Step 6: Perform high-temperature heat treatment on the dried composite material to obtain oxide nanofiber porous thermal protection material.

[0020] Further, in step 3, the molar ratio of each component in the nanoparticle precursor is: lipids / organic alkoxides / inorganic salts: anhydrous ethanol: deionized water = 1:(0.01~20):(0.1~20).

[0021] Furthermore, in step 3, the nanoparticle precursor is one or more of ZrO2, Y2O3, TiO2, MgO, SiO2, and Al2O3.

[0022] Furthermore, in step 5, the solution pressure of the nanoparticle precursor is 0.1–3 MPa.

[0023] Furthermore, in step 6, the high-temperature heat treatment is carried out at a temperature of 600–1200℃ for a time of 0.5–12 hours.

[0024] (3) Beneficial effects

[0025] In summary, this invention achieves excellent high-temperature resistance, thermal insulation, and toughness through high-strength composite of nano-fibers and micro-fibers. The mechanical properties of the material are further enhanced by impregnation and composite of the preform and nanoparticle precursors, drying, and high-temperature heat treatment. It is a thermal protection material that can simultaneously meet the requirements of thermal insulation, heat resistance, and load-bearing capacity, and is of great significance to the research and application of next-generation thermal protection materials. Attached Figure Description

[0026] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the embodiments of the present invention will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a schematic diagram of the structure of a high-strength oxide nanofiber porous thermal protection material provided in an embodiment of the present invention.

[0028] In the picture:

[0029] 1-Nanoscale oxide fiber layer; 2-Micron-scale oxide fiber layer; 3-Nano particles; 4-Interpenetrating network region. Detailed Implementation

[0030] The embodiments of the present invention will be further described in detail below with reference to the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present invention by way of example, but should not be used to limit the scope of the present invention. That is, the present invention is not limited to the described embodiments, and any modifications, substitutions and improvements to the parts, components and connection methods are covered without departing from the spirit of the present invention.

[0031] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.

[0032] In the description of this invention, it should be understood that the terms "upper," "lower," "front," "rear," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of this invention is in use, or the orientation or positional relationship commonly understood by those skilled in the art. They are only used to facilitate the description of this invention and to simplify the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0033] Figure 1 This is a schematic diagram of the structure of a high-strength oxide nanofiber porous thermal protection material provided in an embodiment of the present invention. The thermal protection material may include a nano-scale oxide fiber layer 1 and a micro-scale oxide fiber layer 2. The nano-scale oxide fiber layer 1 is laid flat on the surface of the micro-scale oxide fiber layer 2 and forms an interpenetrating network structure. Both the nano-scale oxide fiber layer 1 and the micro-scale oxide fiber layer 2 contain nanoparticles 3 inside.

[0034] In the above embodiments, the high-strength composite of nanoscale and microscale fiber materials endows the material with excellent high-temperature resistance, thermal insulation, and toughness. The multi-level combination of materials of different scales enhances mechanical properties, and the combination of nanoscale, microscale, and nanoparticles further improves the material's mechanical properties. As an optional embodiment, the fibers in the nanoscale oxide fiber layer 1 are one or more of mullite nanofibers, SiO2 nanofibers, high-silica nanofibers, and carbon nanofibers.

[0035] As an optional implementation, the fibers in the micron-sized oxide fiber layer 2 are one or more of mullite fibers, alumina fibers, quartz fibers, high silica fibers, aluminum silicate fibers, and glass fibers.

[0036] As an optional implementation, the thickness of the nanoscale oxide fiber layer 1 is 2–10 mm. Experiments have shown that this thickness range yields the best results.

[0037] As an optional implementation, the thickness of the micron-sized oxide fiber layer 2 is 3–20 mm. Experiments have shown that this thickness range yields the best results.

[0038] This invention also provides a method for preparing a high-strength oxide nanofiber porous thermal protection material, which may include the following steps:

[0039] Step 1: The nanoscale oxide fiber is laid flat on the surface of the micron-scale oxide fiber, and the two materials are combined by high-frequency needle punching to form an interpenetrating network structure.

[0040] Step 2: Repeat Step 1 until the thickness of the upper nanofiber reaches the required thickness of the material, and obtain the interpenetrating network structure fiber preform.

[0041] Step 3: Prepare nanoparticle precursors;

[0042] Step 4: Place the interpenetrating network structure fiber preform into a vacuum impregnation mold and evacuate the mold;

[0043] Step 5: Pressurize the nanoparticle precursor into the vacuum impregnation mold containing the interpenetrating network fiber preform, so that it is fully impregnated with the interpenetrating network fiber preform, and continue to evacuate the vacuum until the nanoparticle precursor is cured to obtain the composite material.

[0044] Step 6: The dried composite material is subjected to high-temperature heat treatment to obtain oxide nanofiber porous thermal protection material.

[0045] In the above embodiments, in step 1, the high-frequency needle puncture process has a needle puncture frequency of 4 to 20 Hz, a needle puncture distance of 1 to 15 mm, and a needle puncture depth of 0 to 100%.

[0046] In step 3, the preparation method of the nanoparticle precursor is as follows: Lipids / organic alkoxides / inorganic salts containing the above-mentioned elements are added to a mixed solution of deionized water and anhydrous ethanol in a certain ratio. The pH of the solution is adjusted to 3-5, and the solution is stirred at 10-80℃ for 0.5-15 hours to allow for complete hydrolysis, thereby obtaining the precursor. The solution containing the above-mentioned elements can be one or more of the following: tetraethyl orthosilicate, methyl orthosilicate, polyethoxydisiloxane, methyltriethoxysilane, methyltrimethoxysilane, polysilsesquioxane, γ-glycidyl etheroxypropyltrimethoxysilane, aluminum sec-butoxide, aluminum isopropoxide, nano-Al₂O₃ powder, aluminum nitrate, aluminum chloride, zirconium n-butoxide, yttrium nitrate, and magnesium nitrate.

[0047] The pH of the solution is adjusted to 3-5 using an acid solution, which is selected from one or more of hydrochloric acid, glacial acetic acid, nitric acid, oxalic acid, phosphoric acid, and boric acid.

[0048] In step 6, the drying method can be supercritical drying, freeze drying, vacuum drying, or microwave drying.

[0049] As an optional implementation, in step 3, the molar ratio of each component in the nanoparticle precursor is: lipids / organic alkoxides / inorganic salts: anhydrous ethanol: deionized water = 1:(0.01~20):(0.1~20). Experiments have shown that this component ratio exhibits good results.

[0050] As an optional implementation, in step 3, the nanoparticle precursor is one or a mixture of ZrO2, Y2O3, TiO2, MgO, SiO2, and Al2O3.

[0051] As an optional implementation, in step 5, the solution pressure of the nanoparticle precursor is 0.1–3 MPa. Experiments have shown that the solution pressure within this range yields the best results.

[0052] As an optional implementation method, in step 6, the high-temperature heat treatment temperature is 600–1200℃, and the time is 0.5–12 hours. Experiments have shown that the effect is relatively good within this temperature and time range.

[0053] Example 1

[0054] (1) 200mm×200mm×2mm SiO2 nanofibers were laid flat on the surface of 200mm×200mm×6mm micron mullite fiber felt, and the two materials were composited by high-frequency needle punching process. The needle punching frequency was 8Hz, the needle punching distance was 4mm, and the needle punching depth was 50% of the bottom fiber felt to obtain a nano SiO2 / micron mullite interpenetrating network structure fiber preform.

[0055] (2) Preparation of SiO2 precursor: Tetraethyl orthosilicate was added to a mixed solution of deionized water and anhydrous ethanol. The molar ratio of each component was: tetraethyl orthosilicate: anhydrous ethanol: deionized water = 1:8:2. The pH value was adjusted to 3-5 using hydrochloric acid solution. The mixture was stirred at 40°C for 4 hours to allow it to be fully hydrolyzed and obtain the SiO2 precursor.

[0056] (3) Place the nano-SiO2 / micron mullite interpenetrating network structure fiber preform obtained in step (1) into a vacuum impregnation mold and evacuate for 30 minutes.

[0057] (4) Pressurize the SiO2 precursor solution from step (2) (pressure 2MPa) and inject it into the mold containing the nano-SiO2 / micron mullite interpenetrating network fiber preform in step (4) so ​​that it is fully impregnated with the preform and continue to be vacuumed until the precursor is solidified.

[0058] (5) The interpenetrating network structure fiber preform obtained in step (4) and the nanoparticle composite material are subjected to supercritical drying at a pressure of 18 MPa and a temperature of 120 °C for 24 h.

[0059] (6) The dried material is subjected to heat treatment at a temperature of 1000℃ for 2 hours to obtain a high-strength nano-SiO2 / micron mullite fiber porous thermal protection material.

[0060] Table 1. Performance of the porous thermal protection material of nano-SiO2 / micron mullite fiber in Example 1

[0061]

[0062] Example 2

[0063] (1) 500mm×500mm×5mm SiO2 nanofibers were laid flat on the surface of 500mm×500mm×25mm quartz fiber felt, and the two materials were composited by high-frequency needle punching process. The needle punching frequency was 6Hz, the needle punching distance was 10mm, and the needle punching depth was piercing (100%), to obtain nano SiO2 / micron quartz interpenetrating network structure fiber preform.

[0064] (2) Preparation of Al2O3 and SiO2 composite precursor: Tetraethyl orthosilicate and aluminum sec-butoxide were added to a mixed solution of deionized water and anhydrous ethanol. The molar ratio of each component was: tetraethyl orthosilicate: aluminum sec-butoxide: anhydrous ethanol: deionized water = 1:0.5:8:2. The pH value was adjusted to 3-5 using hydrochloric acid solution. The mixture was stirred at 40°C for 4 hours to allow it to be fully hydrolyzed and obtain the Al2O3 and SiO2 composite precursor.

[0065] (3) Place the nano-SiO2 / micron quartz interpenetrating network structure fiber preform obtained in step (1) into a vacuum impregnation mold and evacuate for 85 minutes.

[0066] (4) Pressurize the Al2O3 and SiO2 composite precursor solution (pressure 0.5MPa) and inject it into the mold of the nano-SiO2 / micron quartz interpenetrating network structure fiber preform placed in step (3) so that it is fully impregnated with the preform and continue to be vacuumed until the precursor is solidified.

[0067] (5) The nanofiber preform / nanoparticle composite material obtained in step (4) is freeze-dried at a freezing temperature of -55℃, a pressure of 0.01MPa, and a time of 96h.

[0068] (6) The dried material is subjected to heat treatment at a temperature of 500℃ for 5 hours to obtain a high-strength nano-SiO2 / micron quartz fiber porous thermal protection material.

[0069] Table 2. Performance of the nano-SiO2 / micron-sized quartz fiber porous thermal protection material in Example 2

[0070]

[0071] Example 3

[0072] (1) 1000mm×1000mm×10mm mullite nanofibers were laid flat on the surface of 1000mm×1000mm×12.5mm micron high silica fiber felt. The two materials were composited by high frequency needle punching process. The needle punching frequency was 8Hz, the needle punching distance was 2mm, and the needle punching depth was 100% to obtain a nano mullite / micron high silica interpenetrating network structure fiber preform.

[0073] (2) Preparation of Al2O3 precursor: Aluminum sec-butoxide was mixed in a ratio of aluminum sec-butoxide: anhydrous ethanol: ethyl acetoacetate: deionized water = 1: 8: 0.5: 12 and stirred at 50°C for 2 h to obtain Al2O3 precursor;

[0074] (3) Place the nano-mullite / micron high silica-oxygen interpenetrating network structure fiber preform obtained in step (1) into a vacuum impregnation mold and evacuate for 60 min.

[0075] (4) Pressurize the Al2O3 precursor solution (pressure 0.8MPa) and inject it into the preform mold containing the nano-mullite / micron high silica-oxygen interpenetrating network structure fiber placed in step (3), so that it is fully impregnated with the preform, and continue to evacuate until the precursor is solidified.

[0076] (5) The nanofiber preform / nanoparticle composite material obtained in step (4) is dried under normal pressure at a temperature of 300°C for 120 hours.

[0077] (6) A high-strength nano-mullite / micron high-silica fiber porous thermal protection material was obtained.

[0078] Table 3 Performance of Example 3 Nanomullite / Micron-high silica fiber porous thermal protection material

[0079]

[0080] It should be noted that the various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referred to mutually. Each embodiment focuses on describing the differences from other embodiments. The present invention is not limited to the specific steps and structures described above and shown in the figures. Furthermore, for the sake of brevity, detailed descriptions of known methods and techniques are omitted here.

[0081] The above are merely embodiments of this application and are not intended to limit the scope of this application. Various modifications and variations can be made to this application by those skilled in the art without departing from the scope of the invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of this application should be included within the scope of the claims of this application.

Claims

1. A method for preparing a high-strength oxide nanofiber porous thermal protection material, wherein the high-strength oxide nanofiber porous thermal protection material comprises a nano-scale oxide fiber layer (1) and a micron-scale oxide fiber layer (2), wherein the nano-scale oxide fiber layer (1) is laid on the surface of the micron-scale oxide fiber layer (2) to form an interpenetrating network structure, and the nano-scale oxide fiber layer (1) and the micron-scale oxide fiber layer (2) both contain nanoparticles (3); characterized in that: The method comprises the following steps: Step 1: Lay the nano-scale oxide fiber on the surface of the micro-scale oxide fiber, and compound the two materials by high-frequency needle punching to form an interpenetrating network structure; Step 2, repeating step 1 until the thickness of the upper layer of nanofibers reaches the required thickness of the material, thereby obtaining an interpenetrating network structure fiber preform; Step 3, preparing nanoparticle precursors; Step 4, placing the interpenetrating network structure fiber preform in a vacuum impregnation mold and evacuating the mold; Step 5, pressurizing the nanoparticle precursor into a vacuum impregnation mold in which the interpenetrating network structure fiber preform is placed, so that the nanoparticle precursor and the interpenetrating network structure fiber preform are fully impregnated, and continuously vacuuming until the nanoparticle precursor is solidified to obtain a composite material; Step 6, subjecting the dried composite material to high-temperature heat treatment to obtain an oxide nanofiber porous thermal protection material; In step 6, the temperature of the high temperature heat treatment is 600-1200° C., and the time is 0.5-12 hours.

2. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: In step 3, the ratio of the components in the nanoparticle precursor is: lipid / organic alcohol salt / inorganic salt: anhydrous ethanol: deionized water = 1: (0.01-20): (0.1-20).

3. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: In step 3, the nanoparticle precursor is a mixture of one or more of ZrO2, Y2O3, TiO2, MgO, SiO2, and Al2O3.

4. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: In step 5, the pressure of the nanoparticle precursor solution is 0.1-3 MPa.

5. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: The fibers in the nano-scale oxide fiber layer (1) are one or more of mullite nanofibers, SiO2 nanofibers, high-silicon nanofibers, and carbon nanofibers.

6. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: The fibers in the micron-sized oxide fiber layer (2) are one or more of mullite fibers, alumina fibers, quartz fibers, high-silica fibers, aluminum silicate fibers, and glass fibers.

7. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: The thickness of the nano-scale oxide fiber layer (1) is 2 to 10 mm.

8. The method for preparing the high-strength oxide nanofiber porous thermal protection material according to claim 1, characterized in that: The thickness of the micron-sized oxide fiber layer (2) is 3 to 20 mm.