A method for preparing a seawater evaporator with a layered porous structure
By using a layered porous carbon material in the seawater evaporator to fill the melamine resin sponge, the problems of complex processes and high cost in traditional seawater desalination technology are solved, and efficient and low-cost seawater desalination effect is achieved.
Patent Information
- Application Number
- CN202211625151.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Traditional seawater desalination technology has problems such as large power consumption, large centralized installation area and frequent maintenance. The production process of existing solar-powered interface evaporation systems is complex, has high cost, and has poor long-term product stability, making it difficult to achieve industrial production.
Using a seawater evaporator preparation method with a layered porous structure, carbon material with a micro/medium/macroporous grading pore structure was prepared by pre-soaking poplar flocs in potassium citrate solution for carbonization and activation, and filling it with In the voids of the melamine resin sponge, a seawater evaporator with excellent light absorption, good water transfer and thermal insulation capabilities are formed.
It has achieved a seawater evaporator with simple production process, low manufacturing cost and good long-term product stability, and can uniformly and efficiently transport seawater to the evaporation interface, significantly improving the efficiency of seawater desalination.
Smart Images

Figure CN115872476B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of seawater desalination, and in particular to a method for preparing a seawater evaporator with a layered porous structure. Background Art
[0002] With the continuous development of economy, the shortage of fresh water resources has become a common problem faced by the global social development. Since seawater accounts for more than 97% of the total water resources on the earth, seawater desalination is considered to be an important way to alleviate the problem of fresh water scarcity. However, the traditional pressure steam distillation, multi-stage flash distillation and reverse osmosis technologies used for fresh water production have problems such as high power consumption, large centralized installation area and frequent maintenance.
[0003] In the existing technology, solar-driven interfacial evaporation technology is an ideal strategy for continuously obtaining fresh water using seawater and solar energy. Compared with traditional seawater desalination technology, the floating structure solar interfacial evaporation system concentrates heat at the liquid-gas interface, which can effectively reduce unnecessary heat loss caused by heating bulk water and achieve a higher conversion efficiency. In order to achieve efficient solar-driven interfacial evaporation, various materials with ingenious structural designs and advanced components have been proposed, such as the construction of three-dimensional non-uniform light absorption surfaces, three-dimensional porous structure photothermal materials, carbon-based materials, polymers, etc. The proposal and application of these materials have greatly promoted the development of seawater desalination technology and provided new ideas for achieving efficient evaporation of seawater. However, the complex production process, high cost and poor long-term stability of the product are still huge challenges for the industrial production of seawater evaporators. Summary of the invention
[0004] In view of the above situation, the purpose of the present invention is to provide a method for preparing a seawater evaporator with a layered porous structure, which has a simple production process, low manufacturing cost and good long-term product stability.
[0005] In order to achieve the above object, the technical solution proposed by the present invention is:
[0006] A method for preparing a seawater evaporator with a layered porous structure comprises the following steps:
[0007] S1 Preparation of poplar fluff loaded with potassium citrate: The collected poplar fluff was cleaned with ethanol and deionized water in turn, and dried in an oven at 60°C overnight to obtain dried poplar fluff; 5 g of dried poplar fluff was soaked in 100 mL of a potassium citrate solution with a molar concentration of 0.5 mol / L, and after it completely absorbed the potassium citrate solution, it was freeze-dried to obtain poplar fluff loaded with potassium citrate;
[0008] S2 Preparation of activated porous carbon: Poplar fluff loaded with potassium citrate is subjected to one-step carbonization and activation under a nitrogen atmosphere, and the product obtained after the one-step carbonization and activation is treated with hydrochloric acid having a molar concentration of 3 mol / L, and washed with deionized water to neutrality to obtain activated porous carbon;
[0009] S3 Preparation of carbonized melamine resin sponge: The melamine resin sponge was ultrasonically cleaned in anhydrous ethanol and deionized water for 30 min, dried at 60 °C for 12 h, and then heated to 600-800 °C at a heating rate of 10 °C / min and annealed for 5 min to obtain a carbonized melamine resin sponge;
[0010] S4: preparing a suspension: adding solid PVA to deionized water, stirring and dissolving at 95 °C to obtain a 10-20 g / L PVA solution, adding the activated porous carbon obtained in S2 to the PVA solution in a certain proportion, stirring for 24 h, and obtaining a suspension;
[0011] S5: preparing a seawater evaporator: immersing the carbonized melamine resin sponge obtained in S3 in the suspension obtained in S4, allowing the carbonized melamine resin sponge to fully absorb the suspension, and then freeze-drying the sponge to obtain a final seawater evaporator.
[0012] Preferably, in S2, the step of carbonizing and activating the poplar fluff loaded with potassium citrate under a nitrogen atmosphere comprises the following steps:
[0013] The poplar fluff loaded with potassium citrate was heated to 400 °C at a heating rate of 10 °C / min under a nitrogen atmosphere and kept warm for 3 h, then heated to 800-950 °C at a heating rate of 10 °C / min and kept warm for 1 h.
[0014] Preferably, in S2, the temperature after heating in the second heating stage is controlled at 850°C.
[0015] Preferably, the temperature after heating in S3 is controlled at 700°C.
[0016] Preferably, the mass ratio of activated porous carbon to PVA in S4 is 7:3.
[0017] The operation steps and parameters not limited in the present invention can be conventionally selected according to the prior art.
[0018] The working principle of the present invention is to pre-soak the collected poplar fluff in a potassium citrate solution and activate it at high temperature under a nitrogen atmosphere to obtain a carbon material (APC) with a micro / meso / macroporous hierarchical pore structure. This is because during the carbonization process, potassium citrate is confined in the fiber cavity of the poplar fluff, and potassium carbonate formed at a relatively low temperature (<650 ° C) gradually decomposes to generate K2O and CO2 through a decomposition reaction: K2CO3 →CO2 + K2O. Between 650 and 850 ° C, most of the CO2 is released at around 830 ° C, and CO2 reacts with carbon to produce a microporous structure. When the temperature is higher than 800 ° C, K2O reacts with carbon: K2O+C →2K + CO, gradually dominating the pore structure and further increasing the pore size. The hierarchical porous structure of APC not only improves the light absorption capacity, but also changes the intermolecular force field between gas, liquid and solid. Subsequently, the prepared APC was filled into the voids of carbonized melamine resin sponge by a simple impregnation method. Melamine resin sponge has the advantages of high porosity, low cost and easy availability. Its interconnected three-dimensional skeleton structure can evenly and efficiently transport seawater to the evaporation interface, thereby producing a seawater evaporator with excellent light absorption, good water transport and heat preservation capabilities.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention provides a preparation method, which has the advantages of simple production process, low manufacturing cost, good long-term product stability, etc., and the seawater evaporator with a layered porous structure prepared by the preparation method of the present invention can uniformly and efficiently transport seawater to the evaporation interface, has excellent light absorption, good water transport and heat preservation capabilities, and can significantly improve the desalination efficiency of seawater. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention in the embodiment;
[0022] Figure 2 Figure a is a scanning electron microscope (SEM) image of the interconnected three-dimensional skeleton structure of the original melamine resin sponge (FM); Figure b is the SEM of the melamine resin sponge (TFM) pyrolyzed at 700 °C; Figure c is the SEM of the directly carbonized poplar fluff carbon tube (PC); Figure d is the SEM of the porous carbon activated by potassium citrate; Figures e and f are both SEMs of the final seawater evaporator (APC@TFM);
[0023] Figure 3 In the figure, a is the Fourier transform infrared spectra (FTIR) of different samples; b is the ultraviolet visible near infrared spectra of different samples; c is the nitrogen adsorption-desorption isotherm of the activated carbon with a hierarchical porous structure; d is the pore size distribution of the activated carbon with a hierarchical porous structure;
[0024] Figure 4 is the contact angle of the final seawater evaporator;
[0025] Figure 5 This is the evaporation performance diagram of different samples. DETAILED DESCRIPTION
[0026] The following will be combined with the attached Figures 1 to 5 The technical scheme of the present invention is clearly and completely described in the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.
[0027] Example 1
[0028] A method for preparing a seawater evaporator with a layered porous structure comprises the following steps:
[0029] S1 Preparation of poplar fluff loaded with potassium citrate: The collected poplar fluff was cleaned with ethanol and deionized water in turn, and dried in an oven at 60°C overnight to obtain dried poplar fluff; 5 g of dried poplar fluff was soaked in 100 mL of a potassium citrate solution with a molar concentration of 0.5 mol / L, and after it completely absorbed the potassium citrate solution, it was freeze-dried for 24 hours to obtain poplar fluff loaded with potassium citrate;
[0030] S2 Preparation of activated porous carbon: The poplar fluff loaded with potassium citrate was heated to 400 °C at a heating rate of 10 °C / min under a nitrogen atmosphere, and kept warm for 3 h, and then heated to 850 °C at a heating rate of 10 °C / min and kept warm for 1 h, for one-step carbonization and activation. The product obtained after one-step carbonization and activation was then treated with hydrochloric acid with a molar concentration of 3 mol / L, and washed with deionized water until neutral, to obtain activated porous carbon, recorded as APC;
[0031] S3 Preparation of carbonized melamine resin sponge: Melamine resin sponge (FM) with a length, width and height of 5 cm, 3 cm and 8 cm respectively was ultrasonically cleaned in anhydrous ethanol and deionized water for 30 min, dried at 60 °C for 12 h, and then heated to 700 °C at a heating rate of 10 °C / min and annealed for 5 min to obtain carbonized melamine resin sponge, denoted as TFM;
[0032] S4: Prepare a suspension: add 0.18 g of solid PVA to 9 mL of deionized water, stir and dissolve at 95 °C to obtain a 20 g / L PVA solution, add 0.21 g of activated porous carbon obtained in S2 to the PVA solution, wherein the mass ratio of activated porous carbon to PVA is 7:3, stir for 24 h, and obtain a suspension;
[0033] S5: preparing a seawater evaporator: immersing the carbonized melamine resin sponge obtained in S3 in the suspension obtained in S4, allowing the carbonized melamine resin sponge to fully absorb the suspension, and then freeze-drying the sponge to obtain a final seawater evaporator, which is recorded as APC@TFM.
[0034] The morphology and microstructure of the intermediate product and the final product in this embodiment were studied using scanning electron microscopy and transmission electron microscopy. Figure 2 As shown, compared with the original sponge MF diagram ( Figure 2 Compared with the TFM graph ( Figure 2 (b) in the figure retains the original interconnected three-dimensional skeleton structure, but becomes a hollow structure during the pyrolysis process; Figure 2 As shown in Figure c, PC has a hollow fiber structure with a smooth surface and a diameter of 5-10 μm; Figure 2 Figure d shows the macroporous structure of APC, with a pore size of about 1~2μm, which is composed of interconnected carbon walls. Figure 2 In the d figure, it can be observed that there are a large number of micropores and mesopores distributed on the APC, which can be further confirmed by BET specific surface area tester. APC was assembled onto the TFM skeleton by a simple impregnation method to obtain APC@TFM. Figure 2 As shown in Figures e and f, APC adheres evenly and tightly to the TMF skeleton.
[0035] Good solar absorption in a wide spectral range is the key to preparing a seawater evaporator with high energy utilization efficiency. The absorption capacity of the sun was investigated in the wavelength range of 220~2600 nm using a UV-visible-near infrared spectrometer. Figure 3 Figure a shows the Fourier transform infrared spectra (FTIR) of different samples. Figure 3 As shown in Figure b, the composite material APC@TFM exhibits the best light absorption capacity (~97%) in a broad spectrum compared to APC and TFM. This is due to the hierarchical porous structure of APC and the three-dimensional skeleton of TFM, which enhance light absorption by increasing the optical path length and reducing the reflectivity. In order to study the light absorption capacity of the evaporator during actual operation, the light absorption of APC@TFM in a water-saturated state was measured. The results show that the absorbance of APC@TFM in a wet water-saturated state is further improved.
[0036] Nitrogen adsorption-desorption analysis was used to further study the specific surface area and pore structure of APC. Figure 3 As shown in Figure c, APC shows a type I physical adsorption isotherm, and the isotherm has a hysteresis phenomenon, indicating that there are a large number of micropores and mesopores. Figure 3As shown in Figure d, the micropores of APC are mainly distributed in the range of 0.7~1.7 nm, and the mesopores are mainly concentrated in the range of 2.7 nm.
[0037] In addition, the hydrophilicity of APC@TFM was characterized by the contact angle. Figure 4 It can be seen that APC@TFM has good hydrophilicity, and water droplets can quickly diffuse to the evaporator surface when the contact angle is 0° within 0.4 s. This is due to the hierarchical porous structure of APC@TFM (rich nano / micro channels) and the inherent hydrophilicity of PVA, which enables water to easily penetrate into the seawater evaporator and transport seawater to the evaporation surface.
[0038] Depend on Figure 5 It can be seen that the seawater evaporator finally prepared has a high efficiency of seawater evaporation rate.
[0039] The working principle of the present invention is to pre-soak the collected poplar fluff in a potassium citrate solution and activate it at high temperature under a nitrogen atmosphere to obtain a carbon material (APC) with a micro / meso / macroporous hierarchical pore structure. This is because during the carbonization process, potassium citrate is confined in the fiber cavity of the poplar fluff, and potassium carbonate formed at a relatively low temperature (<650 ° C) gradually decomposes to generate K2O and CO2 through a decomposition reaction: K2CO3 →CO2 + K2O. Between 650 and 850 ° C, most of the CO2 is released at around 830 ° C, and CO2 reacts with carbon to produce a microporous structure. When the temperature is higher than 800 ° C, K2O reacts with carbon: K2O+C →2K + CO, gradually dominating the pore structure and further increasing the pore size. The hierarchical porous structure of APC not only improves the light absorption capacity, but also changes the intermolecular force field between gas, liquid and solid. Subsequently, the prepared APC was filled into the voids of carbonized melamine resin sponge by a simple impregnation method. Melamine resin sponge has the advantages of high porosity, low cost and easy availability. Its interconnected three-dimensional skeleton structure can evenly and efficiently transport seawater to the evaporation interface, thereby producing a seawater evaporator with excellent light absorption, good water transport and heat preservation capabilities.
[0040] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for preparing a seawater evaporator having a layered porous structure, characterized in that: The steps include: S1 Preparation of poplar fluff loaded with potassium citrate: The collected poplar fluff was cleaned with ethanol and deionized water in turn, and dried in an oven at 60°C overnight to obtain dried poplar fluff; 5 g of dried poplar fluff was soaked in 100 mL of a potassium citrate solution with a molar concentration of 0.5 mol / L, and after it completely absorbed the potassium citrate solution, it was freeze-dried to obtain poplar fluff loaded with potassium citrate; S2 Preparation of activated porous carbon: The poplar fluff loaded with potassium citrate was heated to 400 °C at a heating rate of 10 °C / min under a nitrogen atmosphere, kept warm for 3 h, and then heated to 800-950 °C at a heating rate of 10 °C / min, kept warm for 1 h, for one-step carbonization and activation. The product obtained by one-step carbonization and activation was then treated with hydrochloric acid with a molar concentration of 3 mol / L, and washed with deionized water until neutral to obtain activated porous carbon. S3 Preparation of carbonized melamine resin sponge: The melamine resin sponge was ultrasonically cleaned in anhydrous ethanol and deionized water for 30 min, dried at 60 °C for 12 h, and then heated to 600-800 °C at a heating rate of 10 °C / min and annealed for 5 min to obtain a carbonized melamine resin sponge; S4: preparing a suspension: adding solid PVA to deionized water, stirring and dissolving at 95 °C to obtain a 10-20 g / L PVA solution, adding the activated porous carbon obtained in S2 to the PVA solution in a certain proportion, stirring for 24 h, and obtaining a suspension; Among them, the mass ratio of activated porous carbon to PVA is 7:3; S5: preparing a seawater evaporator: immersing the carbonized melamine resin sponge obtained in S3 in the suspension obtained in S4, allowing the carbonized melamine resin sponge to fully absorb the suspension, and then freeze-drying the sponge to obtain a final seawater evaporator.
2. The method for preparing a seawater evaporator having a layered porous structure according to claim 1, characterized in that: In S2, the temperature after the second heating stage is controlled at 850 °C.
3. The method for preparing a seawater evaporator having a layered porous structure according to claim 1, characterized in that: The temperature after heating in S3 is controlled at 700°C.
Citation Information
Patent Citations
Method for preparing porous carbon micron tube from catkin, poplar seed or phoenix tree seed as raw material
CN102557026A
Solar evaporator with hollow structure, and preparation method and application thereof
CN111170393A
Graphene-attapulgite composite elastic aerogel and application thereof in seawater desalination
CN113908780A
Composite hydrogel sponge, preparation method and application thereof, and solar seawater desalination device
CN114891266A
Preparation method and application of salt-repellent sponge-based / cheap carbon photo-thermal composite material