A ternary polymer scale inhibitor and preparation method thereof
By using ternary polymer scale inhibitors in sewage treatment, combining carboxyl groups, amide groups and organic silicon structures, the problems of single scale inhibitor effect and environmental pollution in the existing technology are solved, and effective inhibition of multiple scales is achieved. and broad-spectrum anti-scaling effect.
Patent Information
- Application Number
- CN202211704067.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Existing antiscalants have a single effect in treating sewage with a high complex ionic composition and contain phosphine compounds, which leads to environmental pollution. There is a lack of broad-spectrum, phosphorus-free and efficient scale inhibitors.
A ternary polymer scale inhibitor is used, which contains carboxyl groups, amide groups and organic silicon structures. It changes the surface properties through silicon-oxygen bonds and is combined with coagulant inhibitors, corrosion inhibitors and decomposers to prepare a scale inhibitor with inhibitory effects on a variety of scales. Antiscalants.
It significantly improves the scale inhibition rate of calcium carbonate, calcium sulfate, calcium phosphate and other scales, expands the scale inhibition range, avoids environmental pollution of phosphine compounds, and provides wider applicability and better purification effect.
Smart Images

Figure CN115872536B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmentally friendly water treatment, and in particular to a ternary polymer scale inhibitor and a preparation method thereof. Background Art
[0002] With the increasing shortage of water resources and the further deterioration of water quality, sewage treatment has become a key research object in the current environmental field. Scaling often occurs in various types of sewage. High scaling will have a serious impact on the instruments and equipment used in most water treatment technologies, thereby affecting the purification effect of sewage. Among the water treatment methods, the reverse osmosis method has the advantages of saving land area, low operating cost, no secondary pollution, stable effluent water quality and high degree of automation control. It is widely used in seawater desalination, water for the pharmaceutical industry, boiler feed water, circulating cooling tower supplementary water and other industries, and has become the main technology for pure water preparation in many industries. However, in the actual operation process, scaling on the surface of the reverse osmosis membrane will seriously affect the normal and stable operation of the system, deteriorate the effluent water quality, shorten the service life of the reverse osmosis membrane, and increase the production cost of the enterprise. Adding scale inhibitors is an important means to prevent scaling.
[0003] Scale inhibitors are a type of agent that can disperse insoluble inorganic salts in water, prevent or interfere with the precipitation and scaling of insoluble inorganic salts on metal surfaces, and maintain good heat transfer effects in metal equipment.
[0004] The use of scale inhibitors effectively solves the scaling problem in industrial cooling and desalination systems, and plays a very important role in increasing the concentration multiple, ensuring the safe and stable operation of industrial production equipment, and solving the problem of global water resource depletion. However, with the increase in the use and discharge of water treatment agents, some environmental problems have also been brought about. Due to the pressure from both environmental protection and use effects, scale inhibitors are driven to develop towards high efficiency and environmental friendliness. Since the early 1930s, when sodium tripolyphosphate and sodium hexametaphosphate were first used to control scaling in urban water supply systems, the development of scale inhibitors has gone through several stages, including inorganic polyphosphates, polyelectrolytes, natural polymers, organic phosphonic acids, polycarboxylic acid copolymers, binary and ternary phosphorus-containing copolymers, and binary and ternary phosphorus-free copolymers, and has developed towards phosphorus-free and non-nitrogen-free environmentally friendly green scale inhibitors.
[0005] However, many sewages now have complex ion components and high content, and many scale inhibitors in the prior art have a single scale inhibition effect. Usually, a certain scale inhibitor has a good scale inhibition effect on only one type of scale in the sewage water body, but it has a poor scale inhibition effect on another type of scale or composite scale. In addition, the existing composite scale inhibitors all contain phosphine compounds, which are easy to pollute the environment and limit their use. Therefore, there is an urgent need for a composite scale inhibitor with good scale inhibition effect, a wide scale inhibition range and no phosphine compounds. Summary of the invention
[0006] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a ternary polymer scale inhibitor with good scale inhibition effect, wide scale inhibition range and no phosphine and a preparation method thereof.
[0007] Technical solution:
[0008] A ternary polymer scale inhibitor, comprising a ternary polymer, an anticoagulant, a corrosion inhibitor, a decomposer and deionized water;
[0009] The ternary polymer structural formula is as follows:
[0010]
[0011] Among them, x:y:z=(5-10):(3-5):(2-4).
[0012] The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains a carboxyl group, an amide group and an organosilicon structure, and has a good inhibitory effect on the formation of calcium carbonate, calcium sulfate and calcium phosphate scales; and by adding the organosilicon structure, through its effect of changing the surface properties and the effect of the silicon-oxygen bond, the scale inhibitor of the present invention is no longer limited to a single scale inhibition mechanism, thereby increasing the scope of application and scale inhibition effect of the scale inhibitor.
[0013] Furthermore, the anticoagulant is selected from one of hydroxysuccinic acid, sodium alkylbenzene sulfonate or polyoxyethylene ether.
[0014] Furthermore, the corrosion inhibitor is selected from one of triethanolamine, sulfonated lignin or benzotriazole.
[0015] Furthermore, the decomposition agent is 2-acrylamide-2-methylpropanesulfonic acid.
[0016] Furthermore, based on the total mass being 100%, the mass percentage of each component is:
[0017]
[0018] The balance was deionized water.
[0019] The method for preparing any one of the above-mentioned ternary polymer scale inhibitors comprises the following steps:
[0020] (1) Adding methacrylic acid chloride and lactamide into a reactor, reacting at 40-70° C. for 8-16 hours under the protection of a polymerization inhibitor, cooling, washing, and drying to obtain methacrylic acid lactamide ester;
[0021] (2) adding maleic anhydride, methacrylic acid lactamide ester, 3-(methacryloyloxy)propyltrimethoxysilane and a solvent into a reactor, reacting at 70-90° C. for 20-40 minutes, adding an initiator, continuing the reaction for 5-8 hours, and removing the solvent to obtain the terpolymer;
[0022] (3) In a container, add the ternary polymer, anticoagulant, corrosion inhibitor, decomposer and deionized water in order according to the mass percentage, and stir for 30-45 minutes to obtain the ternary polymer scale inhibitor.
[0023] In step (1), methacrylic acid lactamide is successfully prepared by reacting methacryloyl chloride with lactamide and grafting amide groups.
[0024] The ternary polymer in the ternary polymer scale inhibitor provided by the invention contains an amide group, and has a good inhibitory effect on the formation of calcium phosphate, iron scale and zinc scale.
[0025] Among them, the reaction process is:
[0026]
[0027] In step (2), maleic anhydride, methacrylate lactamide, and 3-(methacryloyloxy)propyltrimethoxysilane are copolymerized under the action of an initiator to successfully prepare a terpolymer.
[0028] The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains a large number of carboxyl groups, and the carboxyl functional groups are 2+ Mg 2+ Plasma has strong chelating ability and has a strong scale inhibition effect on calcium carbonate and calcium sulfate.
[0029] The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains an organic silicon structure, which can effectively increase the scale inhibition rate for barium strontium ions; a certain siloxy group is introduced into the copolymer molecule to change the hydrophilic and hydrophobic structure of the metal surface, so that the scale cannot be tightly bound to the metal surface, and the silyl methoxy group can be hydrolyzed to form silanol and methanol, wherein the silanol can also form a strong coordination effect with the metal through a coordination bond, so that the scale inhibitor and the metal are tightly bound to form a firm film, and the adhesion and deposition of scale on the metal surface are effectively reduced.
[0030] Furthermore, in the step (1), the polymerization inhibitor is selected from one of hydroquinone, p-methoxyphenol or 2,6-di-tert-butyl-p-cresol.
[0031] Furthermore, in the step (1), the mass ratio of methacryloyl chloride to lactamide is 5:5-8.
[0032] Furthermore, in the step (2), the initiator is selected from one of azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide or tert-butyl perbenzoate; and the solvent is selected from one of anhydrous dimethylformamide or anhydrous dimethyl sulfoxide.
[0033] Furthermore, in the step (2), the mass ratio of maleic anhydride, methacrylic acid lactamide and 3-(methacryloyloxy)propyltrimethoxysilane is (4-7): (6-10): (4-8).
[0034] Beneficial effects:
[0035] (1) The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains a carboxyl group, an amide group and an organosilicon structure, which has a good inhibitory effect on the formation of calcium carbonate, calcium sulfate and calcium phosphate scale; and by adding the organosilicon structure, through its effect of changing the surface properties and the effect of the silicon-oxygen bond, the scale inhibitor of the present invention is no longer limited to a single scale inhibition mechanism, thereby increasing the scope of application and scale inhibition effect of the scale inhibitor.
[0036] (2) The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains a large number of carboxyl groups, and the carboxyl functional groups are 2+ Mg 2+ Plasma has strong chelating ability and has a strong scale inhibition effect on calcium carbonate and calcium sulfate.
[0037] (3) The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains an amide group, which has a good inhibitory effect on the formation of calcium phosphate, iron scale and zinc scale.
[0038] (4) The ternary polymer in the ternary polymer scale inhibitor provided by the present invention contains an organic silicon structure, which can effectively increase the scale inhibition rate for barium strontium ions; certain siloxy groups are introduced into the copolymer molecules to change the hydrophilic and hydrophobic structure of the metal surface, so that the scale cannot be tightly bound to the metal surface, and the silyl methoxy group can be hydrolyzed to form silanol and methanol, among which the silanol can also form a strong coordination effect with the metal through a coordination bond, so that the scale inhibitor and the metal are tightly bound to form a strong film, which effectively reduces the adhesion and deposition of scale on the metal surface. DETAILED DESCRIPTION
[0039] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0040] The commercially available scale inhibitor is WL-602 purchased from Chongqing Wolan Water Treatment Equipment Co., Ltd.; the commercially available terpolymer scale inhibitor is LJ-206 purchased from Jiangsu Piya Industrial Co., Ltd.; the remaining reagents and equipment are conventional reagents and equipment in this technical field.
[0041] Preparation of ternary polymer-1
[0042] (1) Add 5 g of methacrylic acid chloride and 7 g of lactamide to a reactor equipped with heating, stirring, a thermometer, and a reflux condenser, then add 0.01 g of a polymerization inhibitor, hydroquinone, and stir. After reacting at 50° C. for 12 hours, cool to room temperature, wash with 5% sodium carbonate solution (weight percentage concentration) until neutral, stir for 1 hour to decompose the side reaction products and excess methacrylic acid chloride raw material in the reaction solution, wash with water, dry with anhydrous magnesium sulfate, filter, and distill the obtained filtrate under reduced pressure to obtain methacrylic acid lactamide ester;
[0043] (2) In a reactor, 5 g of maleic anhydride, 8 g of methacrylic acid lactamide, 5 g of 3-(methacryloyloxy)propyltrimethoxysilane and 100 ml of anhydrous dimethylformamide solvent were added, and the mixture was reacted at 80° C. for 30 minutes, and then 0.01 g of azobisisobutyronitrile was added. The reaction was continued for 6 hours, and the solvent was removed by distillation under reduced pressure to obtain the terpolymer-1;
[0044] Preparation of ternary polymer-2
[0045] The preparation method is basically the same as that of terpolymer-1, except that the inhibitor in step (1) is changed to p-methoxyphenol; the masses of maleic anhydride, methacrylic acid lactamide ester and 3-(methacryloyloxy)propyltrimethoxysilane in step (2) are changed to 4g, 6g and 8g respectively; the initiator in step (2) is changed to dibenzoyl peroxide, and the solvent is changed to anhydrous dimethyl sulfoxide.
[0046] Preparation of ternary polymer-3
[0047] The preparation method is basically the same as that of terpolymer-1, except that the inhibitor in step (1) is changed to 2,6-di-tert-butyl-p-cresol; the masses of maleic anhydride, methacrylic acid lactamide ester and 3-(methacryloyloxy)propyltrimethoxysilane in step (2) are changed to 7g, 10g and 5g respectively; and the initiator in step (2) is changed to tert-butyl perbenzoate.
[0048] Preparation of ternary polymer-4
[0049] The preparation method is basically the same as that of terpolymer-1, except that step (1) is not performed and methacrylic acid lactamide ester in step (2) is replaced with an equal amount of methacryloyl chloride.
[0050] Preparation of ternary polymer-5
[0051] The preparation is basically the same as that of terpolymer-1, except that in step (2), 3-(methacryloyloxy)propyltrimethoxysilane is replaced by an equal amount of acrylate.
[0052] Example 1
[0053] In a container, add terpolymer, hydroxysuccinic acid, triethanolamine, 2-acrylamide-2-methylpropanesulfonic acid and deionized water in order according to the mass percentage, and stir for 45 minutes to obtain the terpolymer scale inhibitor.
[0054] Wherein, taking the total mass as 100%, the mass percentage of each component is:
[0055]
[0056] The balance was deionized water.
[0057] Example 2
[0058] The same as Example 1, except that the total mass is 100%, and the components and their mass percentages are changed to:
[0059]
[0060] The balance was deionized water.
[0061] Example 3
[0062] The same as Example 1, except that the total mass is 100%, and the components and their mass percentages are changed to:
[0063]
[0064] The balance was deionized water.
[0065] Example 4
[0066] Basically the same as Example 1, except that the terpolymer-1 is replaced by an equal amount of terpolymer-2.
[0067] Example 5
[0068] Basically the same as Example 1, except that the terpolymer-1 is replaced by an equal amount of terpolymer-3.
[0069] Comparative Example 1
[0070] Commercially available antiscalant.
[0071] Comparative Example 2
[0072] Commercially available terpolymer scale inhibitor.
[0073] Comparative Example 3
[0074] Basically the same as Example 1, except that the terpolymer-1 is replaced by an equal amount of terpolymer-4.
[0075] Comparative Example 4
[0076] Basically the same as Example 1, except that the terpolymer-1 is replaced by an equal amount of terpolymer-5.
[0077] Performance Testing
[0078] 1. The scale inhibitors synthesized in Examples 1-5 and Comparative Examples 1-4 were tested for their scale inhibition effects on calcium carbonate scale, calcium sulfate scale and calcium phosphate scale by the calcium carbonate precipitation method:
[0079] Calcium carbonate scale inhibition effect test: calcium ion concentration 250mg / L, bicarbonate ion concentration 732mg / L, test temperature is 80℃.
[0080] Calcium sulfate scale inhibition effect test: calcium ion concentration 6000mg / L, sulfate ion concentration 7000mg / L, test temperature 80℃.
[0081] Calcium phosphate scale inhibition effect test: calcium ion concentration 200mg / L, hydrogen phosphate ion concentration 580mg / L, test temperature is 80℃.
[0082] The results are shown in Table 1:
[0083] Table 1 Comparison of the scale inhibition rates of different scale inhibitors on calcium sulfate, calcium carbonate and calcium phosphate (the amount of scale inhibitor added is 50 mg / L)
[0084] Calcium carbonate scale inhibition rate (%) Calcium sulfate scale inhibition rate (%) Calcium phosphate scale inhibition rate (%) Example 1 96.5 84.7 87.6 Example 2 97.1 85.9 89.8 Example 3 96.4 85.6 87.4 Example 4 98.8 86.2 88.1 Example 5 95.3 84.6 87.3 Comparative Example 1 85.4 63.3 52.7 Comparative Example 2 88.6 78.8 69.7 Comparative Example 3 92.1 81.4 74.6 Comparative Example 4 90.8 80.7 81.2
[0085] According to the comparison of the scale inhibition rates of Examples 1-5 and Comparative Examples 1 and 2, it can be seen that the scale inhibitor provided by the present invention can effectively improve the scale inhibition rate of three types of calcium scales, namely calcium carbonate, calcium sulfate and calcium phosphate, compared with commercially available scale inhibitors, and has a wide scale inhibition range and has excellent scale inhibition ability for various calcium scales.
[0086] According to the comparison of the scale inhibition rates of Examples 1-5 and Comparative Examples 3 and 4, it can be seen that the amide and organosilicon structure contained in the scale inhibitor provided by the present invention can effectively improve the scale inhibition effect on calcium phosphate scale, and can also improve the scale inhibition effect on calcium carbonate and calcium sulfate scale.
[0087] 2. The scale inhibitors synthesized in Examples 1-5 and Comparative Examples 1-4 were measured with reference to the petroleum and natural gas industry standard SY / T5673-93 "Performance Evaluation Method of Scale Inhibitors for Oilfields". On the basis of separating the complex ions in the water, the scale inhibition rates of different ions were determined by the weight method and back titration method.
[0088] The simulated formation water ion concentration is as follows:
[0089]
[0090] The scale inhibition results are shown in Table 2:
[0091] Table 2 Comparison of scale inhibition rates of different scale inhibitors for different ions
[0092]
[0093] According to the comparison of the scale inhibition rates of Examples 1-5 and Comparative Examples 1 and 2, it can be seen that the scale inhibitor provided by the present invention can not only effectively improve the scale inhibition effect on calcium and magnesium ions, but also can significantly improve the scale inhibition ability on barium and strontium ions compared with commercially available scale inhibitors, and the scale inhibition range is wider and the effect is better.
[0094] According to the comparison of the scale inhibition rates of Examples 1-5 and Comparative Examples 3 and 4, it can be seen that the amide and silicone structure contained in the scale inhibitor provided by the present invention can effectively improve the scale inhibition ability for calcium and magnesium ions, and also has a strong scale inhibition ability for barium and strontium ions, with a wider scale inhibition range and better effect.
[0095] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A ternary polymer scale inhibitor, characterized in that: Contains terpolymer, anticoagulant, corrosion inhibitor, decomposer and deionized water; The ternary polymer structural formula is as follows: , Among them, x:y:z=(5-10):(3-5):(2-4); The decomposition agent is 2-acrylamide-2-methylpropanesulfonic acid.
2. The ternary polymer scale inhibitor according to claim 1, characterized in that: The anticoagulant is selected from one of hydroxysuccinic acid, sodium alkylbenzene sulfonate or polyoxyethylene ether.
3. The ternary polymer scale inhibitor according to claim 1, characterized in that: The corrosion inhibitor is selected from one of triethanolamine, sulfonated lignin or benzotriazole.
4. The ternary polymer scale inhibitor according to claim 1, characterized in that: Taking the total mass as 100%, the mass percentage of each component is: Terpolymer 15-20% Anticoagulant 3-5% Corrosion inhibitor 1-3% Decomposition agent 1-3% The balance was deionized water.
5. The method for preparing the ternary polymer scale inhibitor according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Add methacrylic acid chloride and lactamide into a reactor, react at 40-70°C for 8-16 hours under the protection of a polymerization inhibitor, cool, wash and dry to obtain methacrylic acid lactamide ester; (2) Add maleic anhydride, methacrylic acid lactamide, 3-(methacryloyloxy)propyltrimethoxysilane and solvent into a reactor, react at 70-90° C. for 20-40 minutes, add an initiator, continue the reaction for 5-8 hours, remove the solvent, and obtain the terpolymer; (3) In a container, add the ternary polymer, anticoagulant, corrosion inhibitor, decomposer and deionized water in order according to their mass percentages, and stir for 30-45 minutes to obtain the ternary polymer scale inhibitor.
6. The method for preparing the ternary polymer scale inhibitor according to claim 5, characterized in that: In the step (1), the polymerization inhibitor is selected from one of hydroquinone, p-methoxyphenol or 2,6-di-tert-butyl-p-cresol.
7. The method for preparing the ternary polymer scale inhibitor according to claim 5, characterized in that: In the step (1), the mass ratio of methacryloyl chloride to lactamide is 5:5-8.
8. The method for preparing the ternary polymer scale inhibitor according to claim 5, characterized in that: In the step (2), the initiator is selected from one of azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide or tert-butyl perbenzoate; and the solvent is selected from one of anhydrous dimethylformamide or anhydrous dimethyl sulfoxide.
9. The method for preparing the ternary polymer scale inhibitor according to claim 5, characterized in that: In the step (2), the mass ratio of maleic anhydride, methacrylate lactamide and 3-(methacryloyloxy)propyltrimethoxysilane is (4-7): (6-10): (4-8).