Coated glass and preparation method thereof and laminated glass
By eliminating the high-temperature pre-sintering step in the preparation of coated glass and embedding the coating layer material during press molding, the problem of poor adhesion between the coating layer and the glass substrate is solved, product quality and yield are improved, and the process flow is simplified.
Patent Information
- Application Number
- CN202211316973.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-26
AI Technical Summary
In traditional coated glass preparation methods, the adhesion between the coating layer and the glass substrate is poor, resulting in product quality defects and reduced yield, and high-temperature sintering affects the flatness of the glass substrate.
The coating layer is formed before the ink layer is sintered, and the coating layer material is embedded into the ink layer during the pressing and molding process. The high-temperature pre-sintering step is eliminated. Magnetron sputtering coating and screen printing technology are used to ensure the tightness between the coating layer and the glass substrate. Good adhesion and flatness.
It improves the adhesion and yield of coated glass, reduces the residual stress and flatness difference caused by sintering, achieves the film removal effect of the shielding layer, simplifies the production process and reduces costs.
Smart Images

Figure CN115872631B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass products, in particular to coated glass and a preparation method thereof and laminated glass. Background Art
[0002] In recent years, due to the continuous growth of automobile sales and the demand for energy-saving, environmentally friendly and diversified functions of automobile glass, coated glass has been widely favored by customers. Coated glass, also known as reflective glass, is a glass surface coated with one or more layers of metal, alloy or metal compound film to change the optical properties of the glass to meet specific requirements.
[0003] Generally, the periphery of coated glass is printed with an ink layer for shading decoration. When preparing coated glass, ink is first printed around the periphery of the glass substrate, and then sintered at high temperature to form an ink layer. After sintering, the glass substrate is washed and then coated. However, high-temperature pre-firing affects the overall flatness of the glass substrate, resulting in poor adhesion between the coating layer and the glass substrate, causing quality defects in coated glass products. Summary of the invention
[0004] Based on this, the present invention provides a coated glass and a preparation method thereof and laminated glass, which can improve the quality defects of coated glass products and increase the yield rate of coated products.
[0005] The first aspect of the invention provides a method for preparing coated glass. The technical solution is as follows:
[0006] A method for preparing coated glass comprises the following steps:
[0007] Providing a glass substrate, coating an ink composition on a peripheral area of the glass substrate, and drying to obtain an ink layer printed edge glass;
[0008] Forming a coating layer on the surface of the ink layer printed edge glass to obtain a glass to be formed;
[0009] The glass to be formed is press-formed. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0010] The ink composition comprises the following components in weight percentage: 70% to 85% ink pigment and 15% to 30% oil agent.
[0011] Wherein, the ink pigment comprises the following components in weight percentage: Bi 2 O 3 20%~50%, SiO 2 15%~35%,CrO3 10%~25%, CuO 0%~10%, ZnO 0%~10%, Na 2 O 0% to 5% and other trace oxides 0% to 3%, the other trace oxides include MgO, Al 2 O 3 , P 2 O 3 , K 2 O and CaO or more.
[0012] Wherein, the particle size of the ink pigment is 5 μm to 20 μm.
[0013] Wherein, the oil agent includes an organic solvent and a resin;
[0014] The organic solvent is one or more of isopropanol, ethyl acetate, toluene and acetone;
[0015] The resin is one or more of acrylic resin, epoxy resin, polyurethane resin and phenolic resin.
[0016] The oil agent further comprises an auxiliary agent, and the auxiliary agent is one or more of glycerin, varnish, antioxidant and defoaming agent.
[0017] The ink composition further comprises the following components in percentage by weight: 1% to 15% of a diluent; the diluent is one or more of terpineol, toluene, isopropyl alcohol and ethyl acetate.
[0018] Before coating the ink composition, the method further comprises washing the glass substrate, wherein the conductivity of the washing water is ≤8us / cm and the temperature is 18°C to 60°C.
[0019] Wherein, the method for applying the ink composition is screen printing, and the printing pressure of screen printing is 60Mpa to 100Mpa.
[0020] Wherein, the viscosity of the ink composition is 10 Pa·s to 15 Pa·s.
[0021] The drying temperature is set to 100° C. to 300° C., and the drying speed is set to 5 m / min to 15 m / min.
[0022] Wherein, the thickness of the ink layer in the ink layer printed edge glass is 14 μm to 30 μm.
[0023] The coating layer is formed by magnetron sputtering, and the vacuum degree of the magnetron sputtering is 1×10 - 3 mbar~1×10 -6 mbar, working pressure is 1×10-2 mbar~1×10 -4 mbar.
[0024] Wherein, the pressing temperature is 500°C to 700°C, and the pressing time is 170s to 250s.
[0025] Wherein, the flatness of the glass substrate in the ink layer printed edge glass is ≤1mm.
[0026] The second aspect of the present invention provides a coated glass. The technical solution is as follows:
[0027] A coated glass comprises a glass substrate, a shielding layer located in a peripheral area of the glass substrate, and a coating layer located in a middle area of the glass substrate, wherein the shielding layer comprises an ink layer and a coating layer material embedded in the ink layer, and the coated glass is manufactured by the above-mentioned method for manufacturing coated glass.
[0028] Wherein, the coating layer includes at least one functional layer and at least two dielectric layers, the functional layer and the dielectric layer are arranged alternately, and the functional layer is located between at least two dielectric layers.
[0029] The functional layer includes at least one of Ag, Au, Cu, Al and their alloys, and the dielectric layer includes AZO, Ti alloy, NbO x 、TiO x 、NiCr、NiCrO x 、ZnAlO x 、ZnO x SnO x At least one of .
[0030] Wherein, the thickness of the coating layer is 100nm-1000nm.
[0031] Wherein, the thickness of the shielding layer is 10 μm to 30 μm.
[0032] The third aspect of the present invention provides a laminated glass. The technical solution is as follows:
[0033] A laminated glass comprises two sheets of glass and an intermediate layer between the two sheets of glass; at least one sheet of glass is selected from the above-mentioned coated glass.
[0034] Compared with the traditional solution, the present invention has the following beneficial effects:
[0035] The inventor of the present invention has found through research that the poor adhesion between the coating layer of the coated glass formed by the traditional method and the glass substrate is related to the fact that the sintering of the ink in the peripheral area affects the flatness of the glass substrate. According to this discovery, in the method for preparing the coated glass of the present invention, the coating layer is formed before the ink layer is sintered, that is, when the coating layer is formed on the surface of the glass substrate, the ink layer is in an unsintered state, so the glass substrate is not affected by the sintering of the ink layer, and the flatness can reach a level of ≤1mm, or even a level of 0mm to 0.5mm, and there is no residual stress generated by sintering. The formed coating layer has good adhesion to the glass substrate, which can improve the quality defects of the coated glass product. After the coating layer is formed, the ink layer is sintered at the temperature of the pressing molding, and the material of the coating layer is embedded in the ink layer, and the coating layer in the peripheral area is disconnected, so that the formed coated glass is obtained, and the film removal effect of the peripheral area is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0037] Figure 1 This is a schematic flow chart of a method for preparing coated glass according to an embodiment of the present invention;
[0038] Figure 2 A schematic diagram of microscopic changes of pigment particles in an ink layer and a coating layer material during a pressing process according to an embodiment of the present invention;
[0039] Figure 3 A front view of the structure of a coated glass according to an embodiment of the present invention;
[0040] Figure 4 The figure is a top view of the structure of the coated glass according to one embodiment of the present invention. DETAILED DESCRIPTION
[0041] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0043] the term
[0044] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0045] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0046] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0047] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0048] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0049] In the present invention, the first feature being "above" or "below" the second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0050] In the present invention, when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may also be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. It should also be understood that when explaining the connection relationship or positional relationship of elements, although not explicitly described, the connection relationship and positional relationship are interpreted as including an error range, which should be within the acceptable deviation range of a specific value determined by those skilled in the art. For example, "approximately", "approximately" or "substantially" may mean within one or more standard deviations, which are not limited here.
[0051] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0052] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0053] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0054] In view of the problem that the coating layer of coated glass formed by the traditional method has poor adhesion to the glass substrate, the present invention provides a method for preparing coated glass.
[0055] See also Figure 1 , is a method for preparing coated glass according to an embodiment of the present invention, comprising the following steps:
[0056] S1. Provide glass substrate
[0057] In this embodiment, the glass substrate is provided with a peripheral region.
[0058] It can be understood that the glass substrate is obtained by laminating, cutting, shaping, edge grinding, washing and drying flat glass.
[0059] Optionally, during washing, cleaning is performed by physical scrubbing with deionized water; the conductivity of the deionized water used is ≤8μs / cm, preferably ≤3μs / cm, and the conductivity of the last deionized water is ≤0.1μs / cm. During washing, the water temperature is 18-60°C, preferably 30-50°C; after washing, the surface of the glass is dried by air knife, and the air knife gas used includes but is not limited to: filtered air, nitrogen, etc.
[0060] S2, coating ink composition, drying
[0061] In this embodiment, the ink composition is coated on the peripheral area of the glass substrate and dried to obtain the ink layer printed edge glass.
[0062] In this embodiment, the color of the ink composition is black, and the peripheral area is coated with the ink composition to play a role of light-shielding decoration.
[0063] Optionally, the viscosity of the ink composition is 10 Pa·s to 15 Pa·s.
[0064] Optionally, the ink composition comprises the following components in weight percentage: 70% to 85% ink pigment and 15% to 30% oil agent.
[0065] Further optionally, the ink pigment includes the following components in weight percentage: Bi 2 O 3 20%~50%, SiO 2 15%~35%,CrO 3 10%~25%, CuO 0%~10%, ZnO 0%~10%, Na 2 O 0% to 5% and other trace oxides 0% to 3%, the other trace oxides include MgO, Al 2 O 3 , P 2 O 3 , K 2 O and CaO or more.
[0066] Further optionally, the particle size of the ink pigment is 5 μm to 20 μm. Compared with the material of the coating layer, the particle size of the pigment particles in the ink is larger, and the pores between the pigment particles can accommodate the material of the coating layer.
[0067] The oil agent includes an organic solvent and a resin;
[0068] The organic solvent is one or more of isopropanol, ethyl acetate, toluene and acetone.
[0069] The resin is one or more of acrylic resin, epoxy resin, polyurethane resin and phenolic resin.
[0070] The oil agent also includes an auxiliary agent, and the auxiliary agent is one or more of glycerin, varnish, antioxidant and defoaming agent.
[0071] The ink composition further comprises the following components in percentage by weight: 1% to 15% of a diluent; the diluent is one or more of terpineol, toluene, isopropyl alcohol and ethyl acetate.
[0072] In this embodiment, the method of applying the ink composition is screen printing, and optionally, the printing pressure of the screen printing is 60Mpa to 100Mpa. Preferably, the printing pressure is 70Mpa to 90Mpa.
[0073] In this embodiment, drying refers to the transformation of the ink composition from a viscous fluid state to a solid state. After the ink composition is dried, an ink layer is formed. At this time, the pigment particles have not shrunk and crystallized, and are in an unsintered state.
[0074] Optionally, the drying temperature is set to 100° C. to 300° C. Preferably, the drying temperature is set to 150° C. to 200° C.
[0075] Optionally, the drying speed is set to 5m / min to 15m / min. Preferably, the drying speed is set to 6m / min to 9m / min.
[0076] Optionally, the thickness of the ink layer in the ink layer printed edge glass is 14 μm to 30 μm.
[0077] Optionally, the flatness of the glass substrate in the ink layer printed edge glass is ≤1 mm. Preferably, the flatness of the glass substrate in the ink layer printed edge glass is 0-0.5 mm.
[0078] S3, coating
[0079] In this embodiment, a coating layer is formed on the surface of the ink layer printed edge glass to obtain the glass to be formed.
[0080] It can be understood that the surface of the ink layer printed glass refers to the surface of the entire ink layer printed glass on the ink layer side.
[0081] Optionally, at least one functional layer and at least two dielectric layers are formed by coating, the functional layers and the dielectric layers are arranged alternately, and the functional layer is located between at least two dielectric layers. The coating process can be designed to form corresponding layers to meet the use requirements and achieve good optical properties and environmental stability of the glass.
[0082] In this embodiment, the functional layer includes at least one of Ag, Au, Cu, Al and their alloys, and the dielectric layer includes AZO, Ti alloy, NbO x 、TiO x 、NiCr、NiCrO x 、ZnAlO x 、ZnO x SnO x At least one of the following. Silver-based coatings have advantages such as good visible light transmittance and infrared reflectivity, meeting the needs of economic value and comfortable in-vehicle environment, and are gradually being used in the field of automotive glass.
[0083] Optionally, the thickness of the coating layer is 100nm-1000nm.
[0084] In this embodiment, the method for forming the coating layer is magnetron sputtering coating. The magnetron sputtering method is used to coat the entire surface (middle area and peripheral area) of the glass substrate, wherein the coating layer is formed on the middle area of the glass substrate. Since the middle area of the glass substrate is not affected by the sintering of the ink in the peripheral area, the flatness can reach a level of ≤1mm, and can even reach a level of 0-0.5mm, thereby reducing the problem of poor adsorption quality of the coating layer caused by the difference in the flatness of the glass substrate. In addition, there is no residual stress caused by sintering on the glass substrate, and the formed coating layer has good adhesion to the glass substrate, which can improve the quality defects of the coated glass product and form a coating layer with high adhesion and high hardness.
[0085] During coating, the ink layer in the peripheral area has not yet been sintered. Compared with the sintered ink layer, it has lower density and adhesion, which puts higher requirements on the coating process. When it is produced on a large scale, the coating line is required to have a high background vacuum and pumping capacity to reduce the impact of surface impurities, water vapor and volatiles on the chamber atmosphere during the sputtering process.
[0086] In this embodiment, the vacuum degree is set to 1×10 -3 mbar~1×10 -6 mbar. The vacuum degree is preferably set to 1×10 - 5 mbar~1×10 -6 mbar. Set the working pressure to 1×10 -2 mbar~1×10 -4 mbar. The preferred working pressure is 1×10 -2 mbar~1×10 -3 mbar.
[0087] Optionally, during magnetron sputtering, O 2 or N 2As the reaction gas, the cathode target is selected from zinc-tin target, aluminum-doped zinc oxide target, silver target, silicon-aluminum target, etc., and the transmission speed is 2m / min.
[0088] S4, compression molding
[0089] The glass to be formed is press-formed. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0090] See also Figure 2 , which is a schematic diagram of the microscopic changes of the pigment particles in the ink layer and the coating layer material during the pressing and molding process of this embodiment, wherein the particle size of the coating layer material is relatively small and is distributed in the gaps between the pigment particles in the ink layer. As the temperature increases, the pigment particles begin to shrink and crystallize, and the coating layer material is completely embedded in the pigment particles, eventually completing the ink sintering. The continuity of the coating layer in the peripheral area is destroyed, and it is disconnected from the coating layer in the middle area, thereby achieving the film removal effect of the shielding layer.
[0091] In this embodiment, through press molding, not only the coated glass is formed, but also the sintering and densification of the ink and the removal of the film in the peripheral area of the coated glass can be completed to form a shielding layer.
[0092] Optionally, the pressing temperature is 500° C. to 700° C., and the pressing time is 170s to 250s.
[0093] Optionally, the shielding layer has a thickness of 10 μm to 30 μm.
[0094] The method for preparing coated glass of this embodiment eliminates the step of sintering the ink layer before coating, and correspondingly eliminates the step of transferring the ink layer printed edge glass to the sintering furnace for pre-sintering. Because the production capacity of glass to be sintered with ink in existing coated products cannot meet the production capacity of the sintering furnace, it is necessary to share the sintering furnace with other non-coated sintered products. Since there is no plan to connect the sintering furnace and the coating line for production, it is necessary to transfer, which causes waste, pollution, and scratches of the finished coated glass, resulting in a decrease in the coating yield. The method for preparing coated glass of this embodiment can avoid the above problems.
[0095] After the ink of this embodiment is dried, the glass surface has a high cleanliness and can be directly processed to the next step. With the above advantages, the step of washing the intermediate product after sintering before coating can be omitted. In the production line, the process flow can be reduced, the cost can be further reduced, and the economic benefits can be improved.
[0096] In this embodiment, after coating, the ink layer is sintered by pressing and molding, so that one process can achieve multiple uses, save the overall process flow, reduce costs, and improve economic benefits.
[0097] S5. Obtain coated glass
[0098] The coated glass formed by the above method can be formed on a glass substrate with good flatness, thereby improving the coating quality and the overall coating yield. In addition, in the ink layer sintering stage after coating, there is no need to put the intermediate product into a sintering furnace for ink layer sintering.
[0099] See also Figure 3 and Figure 4 , are respectively a front view and a top view of the structure of the coated glass 01 obtained in this embodiment, including a glass substrate 10, a shielding layer 30 located in the peripheral area of the glass substrate 10, and a coating layer 20 located in the middle area of the glass substrate 10.
[0100] In this embodiment, the shielding layer includes an ink layer and a coating layer material embedded in the ink layer.
[0101] The present invention also provides a laminated glass. In one embodiment of the present invention, the laminated glass comprises two sheets of glass and an intermediate layer between the two sheets of glass; at least one sheet of glass is selected from the above-mentioned coated glass.
[0102] The laminated glass of this embodiment is formed by laminating and pressing two sheets of glass and an intermediate layer. The preparation of the laminated glass can refer to conventional processes.
[0103] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples, unless otherwise specified, can all be sourced from commercial sources. The instruments used, unless otherwise specified, can all be sourced from commercial sources. The processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0104] Example 1
[0105] This embodiment provides a method for preparing coated glass, the steps are as follows:
[0106] S1. The flat glass is subjected to lamination, cutting, shaping, edge grinding, washing and drying to obtain a glass substrate.
[0107] S2. Printing the ink composition on the peripheral area of the glass substrate obtained in S1 by using a 77T printing screen, and drying it to obtain an ink layer printed edge glass.
[0108] S3, performing magnetron sputtering coating on the ink layer side surface of the ink layer printed edge glass obtained in S2 to form a coating layer on the entire surface, thereby obtaining the glass to be formed.
[0109] S4. The glass to be formed obtained in S3 is subjected to single-piece press molding. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0110] The steps of loading, cutting, shaping, edge grinding, washing and drying are as follows: placing the flat glass on the cutting table, controlling the cutting pressure to 0.32Mpa, the cutting oil pressure to 0.3Mpa, the edge grinding water pressure to 0.35Mpa, the washing water pressure to 0.25Mpa, the water temperature to 45°C, the conductivity to 3μs / cm, and the washing speed to 9m / min. The steps of preparing the ink composition are as follows: taking 75.7% of the ink pigment, 20.3% of the oil agent and 4% of the diluent by weight, wherein the ink pigment includes the following components Bi by weight: 2 O 3 40%, SiO 2 20%, CrO 3 20%, CuO 8%, ZnO 8%, Na 2 O 3% and MgO 1%; the oil agent includes the following weight percentages: isopropyl alcohol 33%, acrylic resin 67%; the diluent is toluene. The components are mixed and stirred at a speed of 300r / min for 10h. The operation steps of printing the ink composition are: pouring the ink composition into a 77T silk screen, setting the printing pressure to 90Mpa, printing the wet material thickness to 22μm, drying the printed ink composition, setting the drying temperature to 180℃, and the drying speed to 9m / min. The steps of magnetron sputtering coating are: Ar is used as the sputtering gas, and the vacuum degree is controlled to 1×10 -5 mbar, working pressure control 10 - 3 mbar. The steps of pressing are: put the product into the pressing furnace, set the temperature to 650°C, the transmission speed to 60mm / s, and the sintering time to 170s.
[0111] Example 2
[0112] This embodiment provides a method for preparing coated glass, the steps are as follows:
[0113] S1. The flat glass is subjected to lamination, cutting, shaping, edge grinding, washing and drying to obtain a glass substrate.
[0114] S2. Printing the ink composition on the peripheral area of the glass substrate obtained in S1 by using a 90T printing screen, and drying it to obtain an ink layer printed edge glass.
[0115] S3, performing magnetron sputtering coating on the ink layer side surface of the ink layer printed edge glass obtained in S2 to form a coating layer on the entire surface, thereby obtaining the glass to be formed.
[0116] S4. The glass to be formed obtained in S3 is subjected to single-piece press molding. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0117] The steps of loading, cutting, shaping, edge grinding, washing and drying are as follows: placing the flat glass on the cutting table, controlling the cutting pressure to 0.32Mpa, the cutting oil pressure to 0.3Mpa, the edge grinding water pressure to 0.35Mpa, the washing water pressure to 0.25Mpa, the water temperature to 45°C, the conductivity to 3μs / cm, and the washing speed to 9m / min. The steps of preparing the ink composition are as follows: taking 75.7% of the ink pigment, 20.3% of the oil agent and 4% of the diluent by weight, wherein the ink pigment includes the following components Bi by weight: 2 O 3 50%、SiO 2 20%, CrO 3 20%, CuO 3%, ZnO 3%, Na 2 O 3% and Al 2 O 3 1%; the oil agent includes the following weight percentages: 33% toluene, 67% epoxy resin; the diluent is isopropanol. The components are mixed and stirred for 10 hours at a speed of 300r / min. The operation steps of printing the ink composition are: pouring the ink composition into a 90T silk screen, setting the printing pressure to 90Mpa, printing the wet material thickness to 18μm, drying the printed ink composition, setting the drying temperature to 180℃, and the drying speed to 9m / min. The steps of magnetron sputtering coating are: Ar is used as the sputtering gas, and the vacuum degree is controlled to 1×10 -5 mbar, working pressure control 10 - 3 mbar. The steps of pressing are: put the product into the pressing furnace, set the temperature to 650°C, the transmission speed to 60mm / s, and the sintering time to 170s.
[0118] Example 3
[0119] This embodiment provides a method for preparing coated glass, the steps are as follows:
[0120] S1. The flat glass is subjected to lamination, cutting, shaping, edge grinding, washing and drying to obtain a glass substrate.
[0121] S2. Printing the ink composition on the peripheral area of the glass substrate obtained in S1 by using a 77T printing screen, and drying it to obtain an ink layer printed edge glass.
[0122] S3, performing magnetron sputtering coating on the ink layer side surface of the ink layer printed edge glass obtained in S2 to form a coating layer on the entire surface, thereby obtaining the glass to be formed.
[0123] S4. The glass to be formed obtained in S3 is subjected to single-piece press molding. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0124] The steps of loading, cutting, shaping, edge grinding, washing and drying are as follows: placing the flat glass on the cutting table, controlling the cutting pressure to 0.32Mpa, the cutting oil pressure to 0.3Mpa, the edge grinding water pressure to 0.35Mpa, the washing water pressure to 0.25Mpa, the water temperature to 45°C, the conductivity to 3μs / cm, and the washing speed to 9m / min. The steps of preparing the ink composition are as follows: taking 75.7% of the ink pigment, 20.3% of the oil agent and 4% of the diluent by weight, wherein the ink pigment includes the following components Bi by weight: 2 O 3 45%、SiO 2 15%, CrO 3 20%, CuO 8%, ZnO 8%, Na 2 O 3% and P 2 O 3 1%; the oil agent includes the following weight percentage components: 33% ethyl acetate and 67% polyurethane resin; the diluent is ethyl acetate. At a speed of 300r / min, the components are mixed and stirred for 10h. The operation steps of printing the ink composition are: pouring the ink composition into a 77T silk screen, setting the printing pressure to 90Mpa, printing the wet material thickness to 22μm, drying the printed ink composition, setting the drying temperature to 180℃, and the drying speed to 9m / min. The steps of magnetron sputtering coating are: Ar is used as the sputtering gas, and the vacuum degree is controlled to 1×10 -5 mbar, working pressure control 10 -3 mbar. The steps of pressing are: putting the product into the pressing furnace, setting the temperature to 650°C, the transmission speed to 60mm / s, and the sintering time to 250s.
[0125] Example 4
[0126] This embodiment provides a method for preparing coated glass, the steps are as follows:
[0127] S1. The flat glass is subjected to lamination, cutting, shaping, edge grinding, washing and drying to obtain a glass substrate.
[0128] S2. Printing the ink composition on the peripheral area of the glass substrate obtained in S1 by using a 77T printing screen, and drying it to obtain an ink layer printed edge glass.
[0129] S3, performing magnetron sputtering coating on the ink layer side surface of the ink layer printed edge glass obtained in S2 to form a coating layer on the entire surface, thereby obtaining the glass to be formed.
[0130] S4. The glass to be formed obtained in S3 is subjected to single-piece press molding. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0131] The steps of loading, cutting, shaping, edge grinding, washing and drying are as follows: placing the flat glass on the cutting table, controlling the cutting pressure to 0.32Mpa, the cutting oil pressure to 0.3Mpa, the edge grinding water pressure to 0.35Mpa, the washing water pressure to 0.25Mpa, the water temperature to 45°C, the conductivity to 3μs / cm, and the washing speed to 9m / min. The steps of preparing the ink composition are as follows: taking 76.4% of the ink pigment, 19.6% of the oil agent and 4% of the diluent by weight, wherein the ink pigment includes the following components Bi by weight: 2 O 3 25%, SiO 2 30%, CrO 3 20%, CuO 10%, ZnO 10%, Na 2 O 3% and K 2 O 2%; the oil agent includes the following weight percentage components: acetone 37% and phenolic resin 63%; the diluent is pine alcohol. At a speed of 300r / min, the components are mixed and stirred for 10h. The operation steps of printing the ink composition are: pouring the ink composition into a 77T silk screen, setting the printing pressure to 90Mpa, printing the wet material thickness to 22μm, drying the printed ink composition, setting the drying temperature to 180℃, and the drying speed to 9m / min. The steps of magnetron sputtering coating are: Ar is used as the sputtering gas, and the vacuum degree is controlled to 1×10 -5 mbar, working pressure control 10 - 3 mbar. The steps of pressing are: put the product into the pressing furnace, set the temperature to 650°C, the transmission speed to 60mm / s, and the sintering time to 170s.
[0132] Example 5
[0133] This embodiment provides a method for preparing coated glass, the steps are as follows:
[0134] S1. The flat glass is subjected to lamination, cutting, shaping, edge grinding, washing and drying to obtain a glass substrate.
[0135] S2. Printing the ink composition on the peripheral area of the glass substrate obtained in S1 by using a 77T printing screen, and drying it to obtain an ink layer printed edge glass.
[0136] S3, performing magnetron sputtering coating on the ink layer side surface of the ink layer printed edge glass obtained in S2 to form a coating layer on the entire surface, thereby obtaining the glass to be formed.
[0137] S4. The glass to be formed obtained in S3 is subjected to single-piece press molding. At the pressing temperature, the ink layer adheres to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer to form a shielding layer in the peripheral area, thereby obtaining a coated glass in which the peripheral area is the shielding layer and the middle area is the coating layer.
[0138] The steps of loading, cutting, shaping, edge grinding, washing and drying are as follows: placing the flat glass on the cutting table, controlling the cutting pressure to 0.32Mpa, the cutting oil pressure to 0.3Mpa, the edge grinding water pressure to 0.35Mpa, the washing water pressure to 0.25Mpa, the water temperature to 45°C, the conductivity to 3μs / cm, and the washing speed to 9m / min. The steps of preparing the ink composition are as follows: taking 72.8% of the ink pigment, 23.2% of the oil agent and 4% of the diluent by weight, wherein the ink pigment includes the following components by weight: 2 O 3 35%, SiO 2 25%, CrO 3 25%, CuO 5%, ZnO 5%, Na 2 O 4% and CaO 1%; the oil agent includes the following weight percentages: toluene 29% and epoxy resin 71%; the diluent is isopropanol. The components are mixed and stirred for 10 hours at a speed of 300r / min. The operation steps of printing the ink composition are: pouring the ink composition into a 77T silk screen, setting the printing pressure to 90Mpa, printing the wet material thickness to 22μm, drying the printed ink composition, setting the drying temperature to 180℃, and the drying speed to 9m / min. The steps of magnetron sputtering coating are: Ar is used as the sputtering gas, and the vacuum degree is controlled to 1×10 -5 mbar, working pressure control 10 - 3 mbar. The steps of pressing are: put the product into the pressing furnace, set the temperature to 650°C, the transmission speed to 60mm / s, and the sintering time to 170s.
[0139] Comparative Example 1
[0140] This comparative example provides a method for preparing coated glass, the steps are as follows:
[0141] S1. Same as Example 1.
[0142] S2. Referring to step S2 of Example 1, after obtaining the ink layer printed edge glass, sintering is completed at a temperature of 650°C.
[0143] S3. Referring to step S3 of Example 1, magnetron sputtering coating is performed on one side of the ink layer of the intermediate product obtained in S2 to form a coating layer on the entire surface, thereby obtaining glass to be formed.
[0144] S4. Referring to step S4 of Example 1, the glass to be formed obtained in S3 is subjected to single-piece pressing and forming.
[0145] The coated glass prepared in comparative example 1 was compared with the coated glass prepared in examples 1, 2, 3, 4, and 5, and the specific tests were as follows: Film surface resistance, the film surface resistance value of the middle area was tested using a Stratometer G handheld non-contact surface resistance tester. Transition resistance, a handheld digital multimeter was used to test the connection resistance between the middle area and the peripheral area, and the distance was controlled at 5 cm. Transmittance and TDS, the middle area was selected, 5 80mm*80mm samples were taken, and the optical properties were tested using a PerkinElmer Lambda 950 UV-visible spectrophotometer. By testing the transmittance T and reflectivity R of the samples, TDS and TTS can be calculated. Hardness, a set of drawing pencils with hardness specifications of 6B to 6H were selected, and a special tool was used to allow the pencil tip to horizontally scratch the film layer of 10 to 20 mm at a speed of 0.5mm / s to 1mm / s. The surface load stress of the film layer was 750±10g. Observe whether there are scratches on the film layer of more than 3mm, and evaluate the hardness of the corresponding film layer. Take five measured values to calculate the average value. The specific test results are shown in Table 1.
[0146] Table 1 Performance comparison table
[0147]
[0148]
[0149] As can be seen from Table 1, in the coated glass prepared by the present invention, the transition resistance between the middle area and the peripheral area is very large, and the peripheral coating layer is disconnected from the coating layer in the middle area, which can achieve the effect of film removal. At the same time, the hardness of the glass substrate in the middle area is relatively large and scratch-resistant, indicating that the adhesion performance is good. In addition, comparing Comparative Example 1 with Examples 1, 2, 3, 4, and 5, the direct solar transmittance TDS and total transmittance TTS of the coated glass prepared by the present invention decrease, and the visible light transmittance is equivalent. Because the glass of Examples 1, 2, 3, 4, and 5 is not subjected to high-temperature pre-sintering treatment before coating, the surface flatness of large-area flat glass is relatively small, which improves the adhesion and density of the film layer and enhances infrared reflection. Therefore, the preparation method of the present invention can simplify the production process, save costs, and improve the yield rate of coated products.
[0150] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0151] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing coated glass, characterized in that: The following steps are involved: A glass substrate is provided, and an ink composition is coated on the peripheral area of the glass substrate, and dried to make the ink composition transform from a viscous flow state to a solid state to obtain an ink layer printed edge glass, wherein the ink composition comprises the following components in weight percentage: 70% to 85% of ink pigment and 15% to 30% of oil agent; Forming a coating layer on the surface of the ink layer printed edge glass to obtain a glass to be formed; The glass to be formed is pressed and formed. At the pressing and forming temperature, the ink layer is sintered and attached to the peripheral area of the glass substrate, and the coating layer material in the peripheral area is embedded in the ink layer, so that the continuity of the coating layer in the peripheral area is destroyed and disconnected from the coating layer in the middle area, forming a shielding layer in the peripheral area, and obtaining a coated glass with the shielding layer in the peripheral area and the coating layer in the middle area.
2. The method for preparing coated glass according to claim 1, characterized in that: The ink pigment includes the following components in weight percentage: Bi2O3 20% to 50%, SiO2 15% to 35%, CrO3 10% to 25%, CuO 0% to 10%, ZnO 0% to 10%, Na2O 0% to 5% and other trace oxides 0% to 3%, wherein the other trace oxides include one or more of MgO, Al2O3, P2O3, K2O and CaO.
3. The method for preparing coated glass according to claim 2, characterized in that: The particle size of the ink pigment is 5 μm to 20 μm.
4. The method for preparing coated glass according to claim 1, characterized in that: The oil agent includes an organic solvent and a resin; The organic solvent is one or more of isopropanol, ethyl acetate, toluene and acetone; The resin is one or more of acrylic resin, epoxy resin, polyurethane resin and phenolic resin.
5. The method for preparing coated glass according to claim 4, characterized in that: The oil agent also includes an auxiliary agent, which is one or more of glycerin, varnish, antioxidant and defoaming agent.
6. The method for preparing coated glass according to claim 1, characterized in that: The ink composition further comprises the following components in percentage by weight: 1% to 15% of a diluent; the diluent is one or more of terpineol, toluene, isopropyl alcohol and ethyl acetate.
7. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: Before coating the ink composition, the method further comprises a step of washing the glass substrate, wherein the conductivity of the washing water is ≤8 us / cm and the temperature is 18° C. to 60° C.
8. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The method for coating the ink composition is screen printing, and the printing pressure of the screen printing is 60Mpa to 100Mpa.
9. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The viscosity of the ink composition is 10 Pa·s to 15 Pa·s.
10. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The drying temperature is set to 100°C to 300°C, and the drying speed is set to 5m / min to 15m / min.
11. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The thickness of the ink layer in the ink layer printed edge glass is 14 μm to 30 μm.
12. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The coating layer is formed by magnetron sputtering coating, and the vacuum degree of magnetron sputtering coating is 1×10 -3 mbar~1×10 -6 mbar, working pressure is 1×10 -2 mbar~1×10 -4 mbar.
13. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The pressing temperature is 500° C. to 700° C., and the pressing time is 170s to 250s.
14. The method for preparing coated glass according to any one of claims 1 to 6, characterized in that: The flatness of the glass substrate in the ink layer printed edge glass is ≤1mm.
15. A coated glass, characterized in that: The invention comprises a glass substrate, a shielding layer located in a peripheral area of the glass substrate, and a coating layer located in a middle area of the glass substrate, wherein the shielding layer comprises an ink layer and a coating layer material embedded in the ink layer, and the coated glass is prepared by the method for preparing coated glass according to any one of claims 1 to 14.
16. The coated glass according to claim 15, characterized in that: The coating layer includes at least one functional layer and at least two dielectric layers. The functional layer and the dielectric layer are arranged alternately, and the functional layer is located between the at least two dielectric layers.
17. The coated glass according to claim 16, characterized in that: The functional layer includes at least one of Ag, Au, Cu, Al, Ag alloy, Au alloy, Cu alloy and Al alloy, and the dielectric layer includes AZO, Ti alloy, NbO x 、TiO x 、NiCr、NiCrO x 、ZnAlO x 、ZnO x SnO x At least one of .
18. The coated glass according to claim 15, characterized in that: The thickness of the coating layer is 100nm-1000nm.
19. The coated glass according to claim 15, characterized in that: The shielding layer has a thickness of 10 μm to 30 μm.
20. A laminated glass, characterized in that: The invention comprises two sheets of glass and an intermediate layer between the two sheets of glass; at least one sheet of glass is selected from the coated glass described in any one of claims 15 to 19.