A kind of fragrant polybutylene succinate blended fiber and preparation method thereof

By combining PBS with copolymerized modified polybutylene succinate and flavor/β-cyclodextrin inclusions, fragrance blended fibers are prepared, which solves the problem that it is difficult to produce fragrance PBS fibers in conventional monofilament spinning equipment. , achieves the long-lasting release of fragrance and improves mechanical properties, and is suitable for a variety of application scenarios.

CN115874311BActive Publication Date: 2024-11-08SHANGHAI CAIYAN IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211444791.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-11-08
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The prior art is difficult to produce fragrance PBS blended fibers with excellent performance through conventional monofilament spinning equipment, and the fragrance substances have poor heat resistance and are easy to volatilize, resulting in a complex preparation process of aromatic fibers.

Method used

Fragrance blended fibers composed of polybutylene succinate (PBS) and copolymerized modified polybutylene succinate, flavor/β-cyclodextrin inclusions and coupling agents are extruded through twin screws Preparation by machine granulation and melt spinning technology ensures uniform dispersion and high compatibility of flavor/β-cyclodextrin inclusions.

Benefits of technology

It achieves uniform dispersion between PBS and fragrance, excellent mechanical properties and long-lasting fragrance release, low production equipment requirements, simple production process, and is suitable for mattresses, mosquito-repellent insect repellent nets and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003949775600000031
    Figure BDA0003949775600000031
Patent Text Reader

Abstract

The present invention relates to a fragrance polybutylene succinate blended fiber and a preparation method thereof. The fragrance polybutylene succinate blended fiber is composed of polybutylene succinate (PBS), copolymerized modified polybutylene succinate (co-PBS), essence / β-cyclodextrin inclusion compound and coupling agent; the essence / β-cyclodextrin inclusion compound is dispersed in the interior and surface of the fragrance polybutylene succinate blended fiber, and the coupling agent exists between the essence / β-cyclodextrin inclusion compound and polybutylene succinate and copolymerized modified polybutylene succinate; the preparation method is as follows: (1) preparing copolymerized modified polybutylene succinate; (2) preparing fragrance masterbatch; (3) preparing PBS / fragrant masterbatch; (4) preparing the dried PBS / fragrant masterbatch into fragrance polybutylene succinate blended fiber. The fragrance polybutylene succinate blended fiber prepared by the present invention has excellent mechanical properties and lasting fragrance release.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional degradable synthetic polymer fibers and relates to a fragrant polybutylene succinate blended fiber and a preparation method thereof. Background Art

[0002] Polybutylene succinate (PBS) is a biodegradable synthetic polymer with good processability and application performance. The softening point of PBS is 101°C. The high softening point enables PBS to meet the heat resistance requirements of common daily products such as tableware and clothing. The melting point of PBS is 114°C, and the processing temperature is 140-260°C. PBS fiber can be made by melt spinning. The PBS fiber produced by Shaoxing Jiuzhou Company has a breaking strength of 2.69 cN / dtex and an elongation at break of 29.73%. It can be made into disposable dry and wet wipes and other "disposable" products (Structure and Mechanical Properties of Bio-based PBS Fibers [J]. Journal of Basic Sciences of Textile Colleges and Universities, 2019, 32(1):6.). As the production and application ends continue to deepen their understanding of PBS fibers, the production and application of PBS fibers will continue to expand.

[0003] Scented fibers can release fragrance and have multiple functions such as pleasant mood and refreshing mind. The preparation methods of scented fibers include post-finishing and spinning addition. The post-finishing process is simple and suitable for a variety of fibers such as cotton, wool, and chemical fiber, but there are problems with poor wash resistance and affecting the feel. Spinning addition is to add fragrance substances to the fiber during the spinning process, which has the advantages of high fragrance content and long release time. The spinning addition method generally uses melt spinning and wet spinning to prepare scented fibers. Fragrance substances have poor heat resistance and are easy to volatilize. Melt spinning to prepare aromatic fibers requires a low melting point polymer as the matrix. The lower melting point and processing temperature of PBS are conducive to the blending of PBS with low boiling point substances such as essential oils. Patent CN202111520805.5 adopts a two-component spinning method to disclose a method for preparing a skin-core structure PBS / plant essential oil fiber. Patent CN202110908241.6 also adopts a two-component spinning method to disclose a method for preparing a skin-core structure or a sea island structure PBS / plant essential oil fiber. The bicomponent spinning method can be used to prepare aromatic fibers with high essential oil content and slow release, but the bicomponent spinning process requires special bicomponent spinning components and the production process is complicated.

[0004] It can be seen that the production of excellent performance scented PBS blended fibers through conventional single-filament spinning equipment is a technical problem waiting for a breakthrough. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems existing in the prior art and to provide a scented polybutylene succinate (PBS) blended fiber and a preparation method thereof, specifically to provide a scented polybutylene succinate blended fiber in which PBS and a scented substance are evenly dispersed and extruded by a conventional single-filament spinning device and a preparation method thereof.

[0006] To achieve the above object, the scheme adopted by the present invention is as follows:

[0007] A fragrance polybutylene succinate blended fiber, which is composed of polybutylene succinate (PBS), copolymerized modified polybutylene succinate (co-PBS), fragrance / β-cyclodextrin inclusion compound and coupling agent;

[0008] The particle size of the fragrance / β-cyclodextrin inclusion complex in the fragrance polybutylene succinate blended fiber is 0.5-2 μm;

[0009] The flavor / β-cyclodextrin inclusion compound is dispersed in the interior and surface of the flavor polybutylene succinate blended fiber, and the coupling agent exists between the flavor / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate.

[0010] The mass ratio of polybutylene succinate and copolymer-modified polybutylene succinate in the aromatic polybutylene succinate blended fiber is 80-100:10-20; if the amount of copolymer-modified polybutylene succinate is lower than this ratio, the compatibility of polybutylene succinate, copolymer-modified polybutylene succinate and flavor / cyclodextrin inclusion complex will not be significantly improved, resulting in a coarser particle size of the flavor / cyclodextrin inclusion complex; if the amount of copolymer-modified polybutylene succinate is higher than this ratio, the crystallinity of the fiber is low, resulting in weaker mechanical properties.

[0011] Polybutylene succinate, the specific brands are Showa Denko 1003MD, Showa Denko 1903MD, PTTMCC BioBPS TM FZ91, PTT MCC BioBPS TM FD92, a type of 803S of Lanshan Tunhe Company;

[0012] The copolymer modified polybutylene succinate is a polybutylene succinate copolymer containing a six-membered ring structural unit.

[0013] As the preferred technical solution:

[0014] The above-mentioned aromatic polybutylene succinate blended fiber, in parts by weight, has the following contents of the components:

[0015] 80-100 parts of polybutylene succinate;

[0016] 10-20 parts of copolymer modified polybutylene succinate;

[0017] 1 to 6 parts of flavor / cyclodextrin inclusion compound;

[0018] 1 to 5 parts of coupling agent.

[0019] In the above-mentioned fragrant polybutylene succinate blended fiber, the fragrance / β-cyclodextrin inclusion compound is a lavender essential oil / β-cyclodextrin inclusion compound, a lemon essential oil / β-cyclodextrin inclusion compound, a cinnamon essential oil / β-cyclodextrin inclusion compound or a grapefruit seed oil / β-cyclodextrin inclusion compound.

[0020] In the above-mentioned fragrant polybutylene succinate blended fiber, the coupling agent is silane coupling agent KH550, silane coupling agent KH560 or silane coupling agent KH570.

[0021] The aromatic polybutylene succinate blended fiber as described above is a monofilament with a diameter of 0.08-1.06 mm, a breaking strength of 1.5-2.2 cN / dtex, a breaking elongation of 35-46%, and an initial modulus of 11.1-15.4 cN / dtex.

[0022] The fragrance polybutylene succinate blended fiber as described above, after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 70-83%;

[0023] The aromatic polybutylene succinate blended fiber is washed according to GB / T 8629-2017 standard, and the elution rate of the aroma is 13-28% after washing 10 times, and the elution rate of the aroma is 32-41% after washing 30 times.

[0024] The present invention also provides a method for preparing the above-mentioned fragrant polybutylene succinate blended fiber, comprising the following steps:

[0025] (1) using Ti(OBu)4 as a catalyst, butanediol, dimethyl succinate and a dimer acid containing a six-membered ring structural unit (trade name: pripol 1006 or pripol 1009) are polymerized to obtain copolymer-modified polybutylene succinate;

[0026] (2) mixing polybutylene succinate, copolymer modified polybutylene succinate, flavor / β-cyclodextrin inclusion compound and coupling agent uniformly, and melt-extruding and granulating the mixture through a twin-screw extruder to obtain a flavor masterbatch;

[0027] (3) mixing polybutylene succinate (PBS) and the fragrance masterbatch with a mixer to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at 80° C. for 5 h using a drying device;

[0028] (4) The dried PBS / fragrance masterbatch is processed by a melt spinning machine according to the process of metering → extrusion → air blowing cooling → one stretching → two stretching to make fragrance polybutylene succinate blended fibers.

[0029] The dimer acid containing a six-membered ester ring structure has a molecular structure as follows:

[0030]

[0031] As the preferred technical solution:

[0032] The method for preparing a fragrant polybutylene succinate blended fiber as described above, step (1) specifically comprises: under the protection of a nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid and Ti(OBu)4 catalyst are stirred to react at a temperature of 180-190°C and normal pressure, and the reaction is terminated when 90% of the methanol is distilled out, and the time is 80-120 minutes; then the temperature is increased to 230°C, the pressure is reduced to 0.1 mbar, and the reaction is terminated when the torque of the agitator is constant, and the reaction time is 100-120 minutes.

[0033] In the preparation method of the fragrant polybutylene succinate blended fiber as described above, the molar ratio of butanediol, dimethyl succinate and dimer acid is 100-140:70-100:5-25, preferably 120:85:15, and the amount of Ti(OBu)4 is 150-250ppm, preferably 200ppm, based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0034] In the method for preparing a scented polybutylene succinate blended fiber as described above, the process parameters in step (4) are: extrusion temperature 150-200°C, blowing temperature 25°C, first stretching draw ratio 2-3 times, second stretching ratio 3-4 times, and second stretching temperature 60-80°C.

[0035] The mechanism of the present invention is as follows:

[0036] β-cyclodextrin is made from starch through the action of microbial enzymes. It is a ring-shaped compound composed of 7 glucose residues connected by β-1,4-glycosidic bonds. β-cyclodextrin is a hollow cylindrical three-dimensional ring structure. The external hydroxyl group has a hydrophilic effect, and the internal CH bond is shielded and has a hydrophobic effect. β-cyclodextrin is often used as an inclusion compound of flavors and fragrances. Compared with unencapsulated flavors, the flavor / β-cyclodextrin inclusion compound has good stability and long-lasting fragrance release.

[0037] The applicant blended PBS with flavor / β-cyclodextrin inclusion complex and prepared flavored PBS fiber. The test found that obvious voids appeared in the fiber cross section, and the particle size of the flavor / β-cyclodextrin inclusion complex was 1 to 4 μm. The coarse particle size of the inclusion complex indicates that the compatibility of the flavor / β-cyclodextrin inclusion complex with PBS is poor, the inclusion complex is difficult to disperse inside the PBS fiber, and obvious agglomeration occurs. As a result, the fiber unevenness is high and the mechanical properties are low. In order to improve the compatibility of the flavor / β-cyclodextrin inclusion complex with PBS, the applicant prepared copolymer modified PBS (co-PBS). Some of the succinic acid structural units of co-PBS are replaced by dimer acid. The aliphatic six-membered ring of dimer acid has a longer side chain, and the -COOR group is also linked by a polyethylene-like segment. In theory, the aliphatic cyclic structure in co-PBS is similar to the molecular structure of the glucose residue in β-cyclodextrin, which is beneficial to improve the compatibility between the two. The experiment found that the particle size of the internal flavor / β-cyclodextrin inclusion complex of the blended fiber containing copolymer-modified PBS was 0.5-2μm, and the fiber cross-section structure was dense. The reduction in the particle size of the flavor / β-cyclodextrin inclusion complex indicates that the dispersion uniformity of the flavor / β-cyclodextrin inclusion complex in co-PBS is improved. Compared with PBS, copolymer-modified PBS has better compatibility with β-cyclodextrin. The good compatibility of copolymer-modified PBS and β-cyclodextrin is conducive to the improvement of the performance of the blended fiber. Compared with the blended fiber without copolymer-modified PBS, the mechanical properties and fragrance release persistence of the blended fiber containing copolymer-modified PBS are better. In addition, silane coupling agent is also added in the preparation process of the fragrance masterbatch. The silane coupling agent reacts with the hydroxyl group of β-cyclodextrin, reducing the polar groups on the surface of the flavor / β-cyclodextrin inclusion complex, further improving the compatibility of the flavor / β-cyclodextrin inclusion complex with PBS and co-PBS.

[0038] Beneficial Effects

[0039] (1) The scented polybutylene succinate blended fiber prepared by the present invention has uniform dispersion of PBS and essence, excellent mechanical properties and long-lasting scent release;

[0040] (2) The aromatic polybutylene succinate blended fiber prepared by the present invention is composed of degradable synthetic polymers or natural polymers, and is an environmentally friendly material. The product is applied to fields that require fragrances, such as mattresses and mosquito repellent nets;

[0041] (3) The present invention prepares the aromatic polybutylene succinate blended fiber through conventional single-filament spinning equipment, which has low production equipment requirements and a simple production process. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0043] The substance information used in the embodiments of the present invention is as follows:

[0044] (1) Dimer acid containing a six-membered ring structural unit: the trade name is Pripol 1009;

[0045] (2) Polybutylene succinate: from Showa Denko Co., trade name 1903MD;

[0046] (3) Lavender essential oil / β-cyclodextrin inclusion complex: Lavender essential oil / β-cyclodextrin inclusion complex was prepared according to the literature (Study on the process of β-cyclodextrin inclusion of lavender essential oil [J]. Food Science and Technology, 2009 (4): 4.), with a wall-core ratio of 8:1;

[0047] (4) Lemon essential oil / β-cyclodextrin inclusion complex: Lemon essential oil / β-cyclodextrin inclusion complex was prepared according to the literature (Optimization of preparation process of lemon essential oil β-cyclodextrin microcapsules [J]. Journal of Weinan Normal University, 2018, 33(4):6.), with a wall-core ratio of 10:1;

[0048] (5) Cinnamon essential oil / β-cyclodextrin inclusion complex: Cinnamon essential oil / β-cyclodextrin inclusion complex was prepared according to the literature (Preparation and sustained release characteristics of cinnamon leaf essential oil / β-cyclodextrin microcapsules [J]. Chemistry and Industry of Forest Products, 2021.), with a wall-core ratio of 4:1;

[0049] (6) Grapefruit seed oil / β-cyclodextrin inclusion complex: Grapefruit seed oil / β-cyclodextrin inclusion complex was prepared according to the literature (Optimization of preparation process of grapefruit seed oil-β-cyclodextrin microcapsules [J]. China Oils and Fats, 2013, 38(10):3.), with a wall-to-oil ratio of 4.5:1.

[0050] The test method used in the embodiments of the present invention is as follows:

[0051] (1) Fiber diameter: The fiber diameter was measured by a micrometer. The diameter of the scented polybutylene succinate blended fiber was 0.08-1.06 mm.

[0052] (2) Breaking strength: GB / T 14344 was used to test the breaking strength of scented polybutylene succinate blended fibers;

[0053] (3) Elongation at break: GB / T 14344 was used to test the elongation at break of scented polybutylene succinate blended fibers;

[0054] (4) Initial modulus: GB / T 14344 was used to test the initial modulus of the scented polybutylene succinate blended fiber;

[0055] (5) Quality retention rate of flavor: Take 10g of the flavored polybutylene succinate blended fiber, use the flavor solvent to elute the flavor in the fiber, and measure the quality of the flavor in the solvent as W1; take another 10g of the flavored polybutylene succinate blended fiber and place it at room temperature for 2 weeks, then use the flavor solvent to elute the flavor in the fiber after 2 weeks, and measure the quality of the flavor in the solvent as W2. The quality retention rate of the flavor in the polybutylene succinate blended fiber after 2 weeks at room temperature is calculated as W2 / W1×100%;

[0056] (6) Elution rate of fragrance: Take 10g of fragrance polybutylene succinate blended fiber, use fragrance solvent to elute the fragrance in the fiber, and measure the mass of fragrance in the solvent as M1; take another 10g of fragrance polybutylene succinate blended fiber and wash it with water 10 times, then use fragrance solvent to elute the fragrance in the fiber after washing 10 times, and measure the mass of fragrance in the solvent as M2; take another 10g of fragrance polybutylene succinate blended fiber and wash it with water 30 times, then use fragrance solvent to elute the fragrance in the fiber after washing 30 times, and measure the mass of fragrance in the solvent as M3. The elution rate of fragrance after washing 10 times is calculated as (1-M2 / M1)×100%, and the elution rate of fragrance after washing 30 times is calculated as (1-M3 / M1)×100%.

[0057] Example 1

[0058] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0059] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing six-membered ring structural units and Ti(OBu)4 were stirred and reacted at 185°C and normal pressure for 100 minutes, then the temperature was increased to 230°C, the pressure was reduced to 0.1 mbar, and the reaction was continued for 110 minutes to obtain copolymer-modified polybutylene succinate;

[0060] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 120:85:15, and the amount of Ti(OBu)4 is 200 ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0061] (2) By weight, 90 parts of polybutylene succinate, 15 parts of the copolymer-modified polybutylene succinate obtained in step (1), 3 parts of lavender essential oil / β-cyclodextrin inclusion compound and 3 parts of silane coupling agent KH550 are stirred and mixed uniformly, and the mixture is melt-extruded and granulated to obtain a fragrance masterbatch;

[0062] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0063] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 175°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 2 times, temperature is 25°C) → two stretching (stretching ratio is 4 times, temperature is 70°C) to prepare a fragrant polybutylene succinate blended fiber.

[0064] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, lavender essential oil / β-cyclodextrin inclusion compound and silane coupling agent KH550; the particle size of the lavender essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 0.7-1.5 μm; the fiber cross-section structure is dense and has no holes; the lavender essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH550 exists between the lavender essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0065] The diameter of the fragrance polybutylene succinate blended fiber is 0.5 mm, the breaking strength is 2.0 cN / dtex, the breaking elongation is 38%, and the initial modulus is 12.4 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 83%; according to GB / T 8629-2017 standard, the fragrance polybutylene succinate blended fiber is washed with water, and the elution rate of the fragrance after washing 10 times is 13%, and the elution rate of the fragrance after washing 30 times is 32%.

[0066] Comparative Example 1

[0067] A method for preparing a scented polybutylene succinate blended fiber is basically the same as that of Example 1, except that step (1) is omitted and copolymer-modified polybutylene succinate is not added in step (2);

[0068] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate and lavender essential oil / β-cyclodextrin inclusion compound; the particle size of the lavender essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 1-4 μm; a large number of holes are present in the fiber cross section, and the hole particle size is 0.05-0.28 μm; the lavender essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and a silane coupling agent KH550 exists between the lavender essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate;

[0069] The diameter of the fragrance polybutylene succinate blended fiber is 0.5 mm, the breaking strength is 1.3 cN / dtex, the breaking elongation is 31%, and the initial modulus is 9.8 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 65%; the fragrance polybutylene succinate blended fiber is washed in accordance with GB / T 8629-2017 standard, and the elution rate of the fragrance after washing 10 times is 37%, and the elution rate of the fragrance after washing 30 times is 43%.

[0070] Comparing Comparative Example 1 with Example 1, it can be found that the breaking strength, breaking elongation and initial modulus of Comparative Example 1 are lower than those of Example 1, the mass retention rate of the flavor in Comparative Example 1 is lower than that in Example 1, and the elution rate of the flavor in Comparative Example 1 is higher than that in Example 1. This is because there is no copolymerized modified polybutylene succinate in the fiber of Comparative Example 1. Therefore, the particle size of the flavor / cyclodextrin inclusion complex in Comparative Example 1 reaches 1-4 μm, indicating that the compatibility of PBS and the flavor / cyclodextrin inclusion complex is poor, and the flavor / cyclodextrin inclusion complex is not a structural component of the fiber that bears tension. The larger particle size of the flavor / cyclodextrin inclusion complex causes a large number of structural weak points in the fiber of Comparative Example 1, resulting in lower mechanical properties of the fiber; in addition, the fiber cross-section of Comparative Example 1 has many holes and a loose fiber structure, which accelerates the release of the flavor. Therefore, the flavor in the fiber of Comparative Example 1 is released quickly and is easy to elute.

[0071] Example 2

[0072] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0073] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing six-membered ring structural units and Ti(OBu)4 were stirred and reacted at 190°C and normal pressure for 80 minutes, then the temperature was increased to 230°C, the pressure was reduced to 0.1 mbar, and the reaction was continued for 100 minutes to obtain copolymer-modified polybutylene succinate;

[0074] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 100:100:5, and the amount of Ti(OBu)4 is 150 ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0075] (2) By weight, 80 parts of polybutylene succinate, 20 parts of the copolymerized modified polybutylene succinate obtained in step (1), 1 part of lemon essential oil / β-cyclodextrin inclusion compound and 1 part of silane coupling agent KH560 are stirred and mixed uniformly, and the mixture is melt-extruded and granulated to obtain a fragrance masterbatch;

[0076] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0077] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 150°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 2 times, temperature is 25°C) → two stretching (stretching ratio is 3.5 times, temperature is 80°C) to prepare a fragrant polybutylene succinate blended fiber.

[0078] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, lemon essential oil / β-cyclodextrin inclusion compound and silane coupling agent KH560; the particle size of the lemon essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 0.5-0.9 μm; the fiber cross-section structure is dense and has no holes; the lemon essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH560 exists between the lemon essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0079] The diameter of the fragrance polybutylene succinate blended fiber is 0.08 mm, the breaking strength is 1.9 cN / dtex, the breaking elongation is 35%, and the initial modulus is 15.4 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 71%; the fragrance polybutylene succinate blended fiber is washed in accordance with GB / T 8629-2017 standard, and the elution rate of the fragrance after washing 10 times is 28%, and the elution rate of the fragrance after washing 30 times is 41%.

[0080] Example 3

[0081] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0082] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing a six-membered ring structural unit and Ti(OBu)4 were stirred and reacted at 185° C. under normal pressure for 120 minutes, then the temperature was increased to 230° C., the pressure was reduced to 0.1 mbar, and the reaction was continued for 120 minutes to obtain copolymer-modified polybutylene succinate;

[0083] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 140:70:25, and the amount of Ti(OBu)4 is 250ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0084] (2) By weight, 85 parts of polybutylene succinate, 13 parts of the copolymerized modified polybutylene succinate obtained in step (1), 2 parts of cinnamon essential oil / β-cyclodextrin inclusion compound and 2 parts of silane coupling agent KH570 are stirred and mixed uniformly, and the mixture is melt-extruded and granulated to obtain a fragrance masterbatch;

[0085] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0086] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 160°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 2.5 times, temperature is 25°C) → two stretching (stretching ratio is 3 times, temperature is 60°C) to prepare a fragrant polybutylene succinate blended fiber.

[0087] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, cinnamon essential oil / β-cyclodextrin inclusion compound and silane coupling agent KH570; the particle size of the cinnamon essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 0.6-1.2 μm; the fiber cross-section structure is dense and has no holes; the cinnamon essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH570 exists between the cinnamon essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0088] The diameter of the fragrance polybutylene succinate blended fiber is 0.55 mm, the breaking strength is 2.2 cN / dtex, the breaking elongation is 39%, and the initial modulus is 11.1 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 78%; the fragrance polybutylene succinate blended fiber is washed in accordance with GB / T 8629-2017 standard, and the elution rate of the fragrance after washing 10 times is 25%, and the elution rate of the fragrance after washing 30 times is 33%.

[0089] Example 4

[0090] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0091] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing six-membered ring structural units and Ti(OBu)4 were stirred and reacted at 180°C under normal pressure for 90 minutes, then the temperature was increased to 230°C, the pressure was reduced to 0.1 mbar, and the reaction was continued for 115 minutes to obtain copolymer-modified polybutylene succinate;

[0092] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 130:90:10, and the amount of Ti(OBu)4 is 180 ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0093] (2) By weight, 92 parts of polybutylene succinate, 16 parts of the copolymerized modified polybutylene succinate obtained in step (1), 4 parts of grapefruit seed oil / β-cyclodextrin inclusion compound and 4 parts of silane coupling agent KH550 are stirred and mixed uniformly, and the mixture is melt-extruded and granulated to obtain a fragrance masterbatch;

[0094] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0095] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 180°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 2.5 times, temperature is 25°C) → two stretching (stretching ratio is 4 times, temperature is 65°C) to prepare a fragrant polybutylene succinate blended fiber.

[0096] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, grapefruit seed oil / β-cyclodextrin inclusion compound and silane coupling agent KH550; the particle size of the grapefruit seed oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 0.9-1.4 μm; the fiber cross-section structure is dense and has no holes; the grapefruit seed oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH550 exists between the grapefruit seed oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0097] The diameter of the fragrance polybutylene succinate blended fiber is 0.71 mm, the breaking strength is 2 cN / dtex, the breaking elongation is 46%, and the initial modulus is 12.8 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 79%; the fragrance polybutylene succinate blended fiber is washed in accordance with GB / T 8629-2017 standard, and the elution rate of the fragrance after washing 10 times is 19%, and the elution rate of the fragrance after washing 30 times is 34%.

[0098] Example 5

[0099] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0100] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing a six-membered ring structural unit and Ti(OBu)4 were stirred and reacted at a temperature of 188° C. and normal pressure for 100 minutes, then the temperature was increased to 230° C., the pressure was reduced to 0.1 mbar, and the reaction was continued for 110 minutes to obtain copolymer-modified polybutylene succinate;

[0101] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 110:80:15, and the amount of Ti(OBu)4 is 220 ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0102] (2) By weight, 95 parts of polybutylene succinate, 18 parts of the copolymer-modified polybutylene succinate obtained in step (1), 5 parts of lavender essential oil / β-cyclodextrin inclusion compound and 5 parts of silane coupling agent KH560 are stirred and mixed uniformly, and the mixture is melt-extruded and granulated to obtain a fragrance masterbatch;

[0103] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0104] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 200°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 3 times, temperature is 25°C) → two stretching (stretching ratio is 3.5 times, temperature is 75°C) to prepare a fragrant polybutylene succinate blended fiber.

[0105] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, lavender essential oil / β-cyclodextrin inclusion compound and silane coupling agent KH560; the particle size of the lavender essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 1.1-1.7 μm; the fiber cross-section structure is dense and has no holes; the lavender essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH560 exists between the lavender essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0106] The diameter of the fragrance polybutylene succinate blended fiber is 0.83 mm, the breaking strength is 1.8 cN / dtex, the breaking elongation is 43%, and the initial modulus is 13.4 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 81%; according to GB / T 8629-2017 standard, the fragrance polybutylene succinate blended fiber is washed with water, and the elution rate of the fragrance is 17% after washing 10 times, and the elution rate of the fragrance is 33% after washing 30 times.

[0107] Example 6

[0108] A method for preparing a scented polybutylene succinate blended fiber, the specific steps are as follows:

[0109] (1) under the protection of nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid containing a six-membered ring structural unit and Ti(OBu)4 were stirred and reacted at 185° C. under normal pressure for 110 minutes, then the temperature was increased to 230° C., the pressure was reduced to 0.1 mbar, and the reaction was continued for 105 minutes to obtain copolymer-modified polybutylene succinate;

[0110] The molar ratio of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit is 125:95:20, and the amount of Ti(OBu)4 is 165 ppm based on the total mass of butanediol, dimethyl succinate and dimer acid.

[0111] (2) mixing 100 parts by weight of polybutylene succinate, 10 parts of the copolymer-modified polybutylene succinate obtained in step (1), 6 parts of lemon essential oil / β-cyclodextrin inclusion compound and 5 parts of silane coupling agent KH570, and melt-extruding and granulating the mixture to obtain a fragrance masterbatch;

[0112] (3) mixing polybutylene succinate with the fragrance masterbatch obtained in step (2) to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 h;

[0113] (4) The dried PBS / fragrant masterbatch obtained in step (3) is processed according to the process path of metering → extrusion (spinneret temperature is 190°C) → air cooling (air cooling temperature is 25°C) → one stretching (stretching ratio is 3 times, temperature is 25°C) → two stretching (stretching ratio is 3 times, temperature is 80°C) to prepare a fragrant polybutylene succinate blended fiber.

[0114] The prepared aromatic polybutylene succinate blended fiber consists of polybutylene succinate, copolymerized modified polybutylene succinate, lemon essential oil / β-cyclodextrin inclusion compound and silane coupling agent KH570; the particle size of the lemon essential oil / β-cyclodextrin inclusion compound in the aromatic polybutylene succinate blended fiber is 1.1-2.0 μm; the fiber cross-section structure is dense and has no holes; the lemon essential oil / β-cyclodextrin inclusion compound is dispersed inside and on the surface of the aromatic polybutylene succinate blended fiber, and the silane coupling agent KH570 exists between the lemon essential oil / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate;

[0115] The diameter of the fragrance polybutylene succinate blended fiber is 1.06 mm, the breaking strength is 1.5 cN / dtex, the breaking elongation is 41%, and the initial modulus is 12.5 cN / dtex; after being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 78%; the fragrance polybutylene succinate blended fiber is washed in accordance with GB / T 8629-2017 standard, and the elution rate of the fragrance after washing 10 times is 23%, and the elution rate of the fragrance after washing 30 times is 37%.

Claims

1. A scented polybutylene succinate blended fiber, characterized in that: It is composed of polybutylene succinate, copolymer modified polybutylene succinate, flavor / β-cyclodextrin inclusion compound and coupling agent; The particle size of the fragrance / β-cyclodextrin inclusion complex in the fragrance polybutylene succinate blended fiber is 0.5~2μm; The flavor / β-cyclodextrin inclusion compound is dispersed in the interior and surface of the flavor polybutylene succinate blended fiber, and the coupling agent exists between the flavor / β-cyclodextrin inclusion compound and the polybutylene succinate and the copolymerized modified polybutylene succinate. The mass ratio of polybutylene succinate to copolymer modified polybutylene succinate in the aromatic polybutylene succinate blended fiber is 80-100:10-20; The copolymer modified polybutylene succinate is a polybutylene succinate copolymer containing a six-membered ring structural unit, which is prepared by polymerizing butanediol, dimethyl succinate and a dimer acid containing a six-membered ring structural unit using Ti(OBu)4 as a catalyst. The trade name of the dimer acid containing a six-membered ring structural unit is pripol 1006 or pripol 1009.

2. The scented polybutylene succinate blended fiber according to claim 1, characterized in that: By weight, the contents of the various components in the aromatic polybutylene succinate blended fibers are as follows: 80-100 parts of polybutylene succinate; 10-20 parts of copolymer modified polybutylene succinate; 1-6 parts of flavor / β-cyclodextrin inclusion compound; 1~5 parts of coupling agent.

3. The scented polybutylene succinate blended fiber according to claim 1, characterized in that: The essence / β-cyclodextrin inclusion compound is a lavender essential oil / β-cyclodextrin inclusion compound, a lemon essential oil / β-cyclodextrin inclusion compound, a cinnamon essential oil / β-cyclodextrin inclusion compound or a grapefruit seed oil / β-cyclodextrin inclusion compound.

4. The scented polybutylene succinate blended fiber according to claim 1, characterized in that: The coupling agent is silane coupling agent KH550, silane coupling agent KH560 or silane coupling agent KH570.

5. The scented polybutylene succinate blended fiber according to claim 1, characterized in that: The diameter of the aromatic polybutylene succinate blended fiber is 0.08-1.06 mm, the breaking strength is 1.5-2.2 cN / dtex, the breaking elongation is 35-46%, and the initial modulus is 11.1-15.4 cN / dtex.

6. The scented polybutylene succinate blended fiber according to claim 5, characterized in that: After being placed at room temperature for 2 weeks, the mass retention rate of the fragrance in the fragrance polybutylene succinate blended fiber is 70-83%; The fragrance polybutylene succinate blended fiber was washed according to GB / T 8629-2017 standard. After 10 washings, the elution rate of the fragrance was 13-28%, and after 30 washings, the elution rate of the fragrance was 32-41%.

7. A method for preparing a scented polybutylene succinate blended fiber as claimed in any one of claims 1 to 6, characterized in that The steps include: (1) Using Ti(OBu)4 as a catalyst, copolymer-modified polybutylene succinate was prepared by polymerization of butanediol, dimethyl succinate and dimer acid containing a six-membered ring structural unit; (2) mixing polybutylene succinate, copolymer modified polybutylene succinate, flavor / β-cyclodextrin inclusion compound and coupling agent uniformly, and melt-extruding and granulating the mixture to obtain flavor masterbatch; (3) mixing polybutylene succinate with the fragrance masterbatch to obtain PBS / fragrance masterbatch, and then drying the PBS / fragrance masterbatch at a temperature of 80° C. for 5 hours; (4) The dried PBS / fragrance masterbatch is processed into fragrance polybutylene succinate blended fibers according to the process path of metering → extrusion → air cooling → one-step stretching → two-step stretching.

8. The method for preparing a scented polybutylene succinate blended fiber according to claim 7, characterized in that: Step (1) is specifically as follows: under the protection of a nitrogen atmosphere, butanediol, dimethyl succinate, dimer acid and Ti(OBu)4 are stirred and reacted at a temperature of 180-190°C and normal pressure for 80-120 minutes; then the temperature is increased to 230°C, the pressure is reduced to 0.1 mbar, and the reaction is continued for 100-120 minutes.

9. The method for preparing a scented polybutylene succinate blended fiber according to claim 8, characterized in that: The molar ratio of butanediol, dimethyl succinate and dimer acid is 100-140:70-100:5-25; based on the total mass of butanediol, dimethyl succinate and dimer acid, the dosage of Ti(OBu)4 is 150-250ppm.

10. The method for preparing a scented polybutylene succinate blended fiber according to claim 7, characterized in that: The process parameters in step (4) are: extrusion temperature 150~200℃, blowing temperature 25℃, first stretching multiple 2~3 times, second stretching multiple 3~4 times, second stretching temperature 60~80℃.

Citation Information

Patent Citations

  • Plant essential oil-containing poly (butylene succinate) composite fiber and preparation method thereof

    CN113802216A

  • Aromatic polypropylene fiber and preparation method thereof

    CN105002584A

  • Composite fiber containing capsules and preparation method thereof

    CN105155032A

  • Plant essence PBS (Phosphate Buffer Solution) master batch and method for preparing skin-core structure fiber by using same

    CN114149663A