A capacitive deionization system capable of strengthening its electrode materials with the help of electrolyte
By using sodium ferricyanide solution to strengthen the activated carbon electrode and ammonium chloride solution to strengthen the MnO2 electrode in the CDI system, the hydrogen bond breaking and electroadsorption mechanisms are used to solve the problem of low desalination in CDI technology and achieve efficient seawater desalination. , and simplifies the preparation process to facilitate industrial application.
Patent Information
- Application Number
- CN202211665468.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The existing capacitive deionization (CDI) technology has a low desalination capacity in seawater desalination, and the research on electrode materials and electrolytes has not been in-depth, resulting in limited desalination performance.
By using sodium ferricyanide solution to strengthen the activated carbon electrode and ammonium chloride solution to strengthen the MnO2 electrode in the anode chamber and cathode chamber respectively, hydrogen bond breaking and electroadsorption mechanisms are used to collaboratively adsorb sodium ions and chloride ions to improve desalination performance.
It significantly improves the desalination capacity and cycle stability of the CDI system. It shows excellent desalination performance especially in high-concentration salt water environments, has large-scale application potential, and simplifies the preparation process to facilitate industrial promotion.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of salt water desalination, and relates to a capacitive deionization system capable of strengthening its electrode material with the aid of electrolyte. Background Art
[0002] Given the abundant seawater and brackish water resources on the earth, converting seawater into fresh water through desalination technology is an effective way to solve this problem. Common seawater desalination strategies usually include reverse osmosis, thermal distillation, electrodialysis and capacitive deionization (CDI). Reverse osmosis, thermal distillation and electrodialysis have been widely used around the world, and demand is still growing. However, these three methods are accompanied by high energy consumption. As an alternative solution, CDI is easy to operate and environmentally friendly, and its low energy consumption provides a sustainable future for seawater desalination. CDI removes ions from brine based on electrical absorption on the electrode surface. The ions are collected and stored in the double layer, but its low capacitance leads to relatively low desalination.
[0003] After a lot of research, it was found that hybrid capacitive deionization (HCDI) has a higher desalination capacity, in which the Faraday electrode captures sodium ions on one side and the carbon-based material is located on the other side to physically absorb chloride ions, but it still has some thresholds because its desalination method relies on the removal of ions through the electrical adsorption of the bulk material and the Faraday reaction. Therefore, in order to increase the desalination capacity, it is necessary to break these thresholds through the research and improvement of electrode materials and electrolytes. At present, no researchers have studied its threshold and its performance improvement through electrolytes. Summary of the invention
[0004] The present invention aims to provide a capacitive deionization system that can strengthen its electrode material with the help of electrolyte to overcome the problems mentioned in the background technology. The system includes an anode chamber, a cathode chamber and a brine chamber. The sodium ferrocyanide solution in the cathode chamber is used to strengthen the activated carbon electrode to construct a functional interface to synergistically adsorb more sodium ions, and the ammonium chloride solution in the anode chamber is used to strengthen the MnO 2 The electrodes cause hydrogen bonds to break and synergistically adsorb more chloride ions, thereby improving the desalination performance of CDI.
[0005] The technical solution of the present invention is as follows:
[0006] A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte comprises an anode chamber, a cathode chamber and a brine chamber, wherein an anion exchange membrane close to the anode chamber and a cation exchange membrane close to the cathode chamber are arranged between the anode chamber and the cathode chamber, a manganese dioxide electrode sheet is arranged in the anode chamber and is injected with an ammonium chloride solution with a concentration of 0.01 mol / L, and an activated carbon electrode sheet is arranged in the cathode chamber and is injected with a sodium ferrocyanide solution with a concentration of 0.01 mol / L; two adjacent ion exchange membranes in the cation exchange membrane and the anion exchange membrane pair are separated by a chamber to form a brine chamber, and the brine chamber forms a closed loop using a silicone tube; the manganese dioxide electrode sheet is connected to the activated carbon electrode sheet through a wire via an external voltage, and the anode chamber and the cathode chamber are connected using a silicone tube to form a closed loop.
[0007] As a limitation of the present invention:
[0008] (i) The manganese dioxide electrode sheet is prepared in the following steps:
[0009] S1. Preparation of manganese dioxide with ammonium ion hydrogen bond pre-intercalation
[0010] S11, dissolving sodium permanganate and ammonium sulfate in deionized water to form sodium permanganate solution and ammonium sulfate solution, respectively, mixing the sodium permanganate and ammonium sulfate solutions at a molar ratio of 2:1 and stirring them magnetically to obtain a mixed solution;
[0011] S12, transferring the obtained mixed solution to a reaction kettle and reacting it at 170-190° C. for 16 h, and cooling it to room temperature after the reaction is completed to obtain a suspension;
[0012] S13, centrifuging and washing the suspension three times respectively, and then placing the solid product in a freeze drying oven for freeze drying to obtain α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation;
[0013] S2. Preparation of manganese dioxide electrode sheet
[0014] The product prepared in step S1 was ground into powder, and the powder was evenly mixed with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, and then anhydrous ethanol was added to the mixture, stirred for 20 minutes to obtain a slurry mixture, and the slurry mixture was evenly applied on a graphite plate, and dried at 80° C. to obtain a manganese dioxide electrode sheet.
[0015] (ii) The activated carbon electrode sheet is prepared in the following steps:
[0016] The activated carbon was ground into powder and mixed evenly with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, and then anhydrous ethanol was added to the mixture and stirred for 20 minutes to obtain a slurry mixture. The slurry mixture was evenly applied on a graphite plate and dried at 80°C to obtain an activated carbon electrode sheet.
[0017] As a further limitation of the present invention:
[0018] (i) In step S13, the freeze-drying temperature is -60°C and the time is 12 hours.
[0019] The freeze-drying process affects the volatilization rate of water in the material and the strength of the material. Through freeze-drying, its volume remains almost unchanged, the original pore structure is maintained, and concentration does not occur. The special pore structure not only ensures its stability, but also further promotes charge transfer.
[0020] (ii) In step S2, the mass ratio of the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation layer to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone is 20:8.6:5:7.5.
[0021] The mass ratio of the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation layer to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone in the present invention affects the conductivity and ion diffusion of the active material, and further affects the desalination performance and rate performance of the active material.
[0022] (iii) In step S2, the slurry mixture is evenly applied on the graphite plate with a thickness of 0.3-0.5 mm.
[0023] As a further limitation of the present invention:
[0024] (i) The mass ratio of activated carbon to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone is 20:8.6:5:7.5.
[0025] (ii) The slurry mixture is evenly applied on the titanium plate with a thickness of 0.3-0.5 mm.
[0026] The present invention also has a limitation that the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation is in the form of nanorods with a pore diameter of 50 nm. This special pore structure is beneficial for expanding the contact area between the electroactive material and the electrolyte ammonium ions, promoting the storage and diffusion of ammonium ions, and alleviating the structural changes caused by ion insertion / ejection during the discharge / charge process. The α-phase manganese dioxide with ammonium ion pre-intercalation of a smaller molar mass has hydrogen bonds formed between ammonium ions and oxygen atoms, and the strong bond energy prevents structural collapse, and acts as a "structural column" to stabilize the pore structure and provide high cycle performance.
[0027] The present invention provides a capacitive deionization system capable of strengthening its electrode material with the help of electrolyte, wherein the activated carbon electrode is strengthened with sodium ferrocyanide solution in the cathode chamber to synergistically adsorb more sodium ions, and the ammonium chloride solution in the anode chamber is strengthened with MnO 2 The electrodes synergistically adsorb more chloride ions, thereby improving the desalination performance of the system. Specifically, in the anode chamber, while the activated carbon uses the double electric layer to adsorb sodium ions, sodium ferrocyanide undergoes a reduction reaction. The sodium ferrocyanide and the activated carbon electrode sheet increase the contact area and effectively construct a functional interface, thereby synergistically adsorbing more sodium ions; in the cathode chamber, because of the use of ammonium ion hydrogen bond pre-intercalated α-phase manganese dioxide electrode sheets, hydrogen bonds will form between ammonium ions and manganese dioxide to promote charge transfer and further stabilize the structure. Due to its special structure, during the electrolysis process, manganese dioxide with ammonium ion hydrogen bond pre-intercalation uses the breaking of hydrogen bonds in the ammonium chloride electrolyte to transfer a large number of electrons to adsorb chloride ions. This is because the breaking of hydrogen bonds can transfer more electrons, allowing it to adsorb more chloride ions, thereby achieving a significant desalination performance.
[0028] In the electrolysis system of the present invention, the concentrations of ammonium chloride in the anode chamber and sodium ferrocyanide in the cathode chamber are also relatively important. The best effect is achieved when the electrolyte concentration is 0.01 mol / L. When the concentration is lower than this, the performance will be reduced due to insufficient ferrocyanide reducing ability and insufficient number of broken hydrogen bonds. When the concentration is too high, it will not only lead to waste of electrolyte, but also may cause further performance degradation due to increased system resistance due to ion polarization of the intermediate salt solution. Most importantly, sodium ferrocyanide will eventually not only cause environmental impacts of harmful chemicals, but also lead to high maintenance costs.
[0029] The above technical solution of the present invention is taken as a whole, and each step is closely related and cannot be separated.
[0030] After adopting the above technical solution, the beneficial effects achieved by the present invention are as follows:
[0031] 1. The preparation method is simple, the process is easy to control, and it is easy to promote and apply industrially. This systematic improvement will make the CDI system practical in subsequent research.
[0032] 2. The system exhibits excellent desalination performance in high-concentration salt water or even seawater environments, and has great potential for large-scale desalination.
[0033] The specific implementation of the present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is an X-ray diffraction pattern of manganese dioxide with ammonium ion hydrogen bond pre-intercalation;
[0035] Figure 2This is the infrared spectrum of manganese dioxide with ammonium ion hydrogen bond pre-intercalation;
[0036] Figure 3 This is a transmission electron microscopy image of manganese dioxide with ammonium ion hydrogen bond pre-intercalation;
[0037] Figure 4 The desalination performance diagrams of CDI system and HCDI of electrolyte-enhanced electrode materials at different voltages;
[0038] Figure 5 Desalination principle of CDI system with electrolyte-enhanced electrode materials;
[0039] Figure 6 The CV diagram of sodium ferrocyanide enhanced activated carbon electrode and activated carbon electrode;
[0040] Figure 7 The CV diagram of manganese dioxide electrode strengthened with ammonium chloride solution and manganese dioxide electrode;
[0041] Figure 8 It is a desalination performance cycle diagram of the desalination system CDI of the present invention at a voltage of 1.2V. DETAILED DESCRIPTION
[0042] In the following examples, the reagents described are all commercially available unless otherwise specified, and the following experimental methods and detection methods are all based on existing experimental methods and detection methods unless otherwise specified.
[0043] Example 1 A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte
[0044] The present embodiment is a capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte, the system comprising an anode chamber, a cathode chamber and a brine chamber, a cation exchange membrane close to the anode chamber and an anion exchange membrane close to the cathode chamber are arranged between the anode chamber and the cathode chamber, a manganese dioxide electrode sheet is arranged in the anode chamber and is injected with a 0.01 mol / L ammonium chloride solution (as an electrolyte), an activated carbon electrode sheet is arranged in the cathode chamber and is injected with a 0.01 mol / L sodium ferrocyanide solution (as an electrolyte); a chamber is separated between two adjacent ion exchange membranes in the cation exchange membrane and the anion exchange membrane, forming a brine chamber (the brine chamber contains brine to be desalted), and the brine chamber forms a closed loop using a silicone tube. The manganese dioxide electrode sheet is connected to the activated carbon electrode sheet through a wire via an external voltage, and the anode chamber and the cathode chamber are connected using a silicone tube to form a closed loop.
[0045] 1. The manganese dioxide electrode sheet used in the above system is prepared in the following steps:
[0046] S1. Preparation of manganese dioxide with ammonium ion hydrogen bond pre-intercalation
[0047] S11, dissolving sodium permanganate and ammonium sulfate in deionized water to form sodium permanganate solution and ammonium sulfate solution, respectively, mixing the sodium permanganate and ammonium sulfate solutions at a molar ratio of 2:1 and stirring them magnetically to obtain a mixed solution;
[0048] S12, transferring the obtained mixed solution to a reaction kettle and reacting it at 170° C. for 16 h, and cooling it to room temperature after the reaction is completed to obtain a suspension;
[0049] S13. The suspension was centrifuged and washed with water three times respectively, and then the solid product was placed in a freeze drying oven and freeze-dried at a temperature of -60°C for 12 hours to obtain α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation. The α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation was in the shape of nanorods with a pore diameter of 50 nm. Figure 1 and Figure 2 They are the X-ray diffraction diagram and infrared spectrum diagram of the prepared manganese dioxide with this structure. Figure 1 Provides information about the crystal structure of the material, all diffraction can be attributed to α-MnO 2 (JCPDS card number 44-0141). Figure 2 Medium wave number 1400cm -1 The peak is attributed to the NH in-plane bending vibration, 2850 cm -1 and 2920cm -1 The peaks are the stretching vibrations of NH…O and NH, which are the evidence of the hydrogen bond formation by ammonium intercalation. These two characteristics prove the successful synthesis of manganese dioxide with ammonium ion hydrogen bond pre-intercalation. Figure 3 3 is a transmission electron microscope image of the product, from which it can be seen that the synthesized manganese dioxide has a nanorod morphology and shows a one-dimensional shape with a flat end of the nanorod.
[0050] S2. Preparation of manganese dioxide electrode sheet
[0051] The product prepared in step S1 is ground into powder, and the powder is evenly mixed with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, wherein the mass ratio of α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone is 20:8.6:5:7.5; then anhydrous ethanol is added to the mixture, stirred for 20 minutes to obtain a slurry mixture, the slurry mixture is evenly applied on a graphite plate with a thickness of 0.3-0.5 mm, and dried at 80° C. to obtain a manganese dioxide electrode sheet.
[0052] 2. The activated carbon electrode sheet used in the above system is prepared in the following steps:
[0053] The activated carbon was ground into powder, and the powder was evenly mixed with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, wherein the mass ratio of the activated carbon to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone was 20:8.6:5:7.5; then anhydrous ethanol was added to the mixture, stirred for 20 minutes to obtain a slurry mixture, the slurry mixture was evenly applied on a graphite plate with a thickness of 0.3-0.5 mm, and dried at 80° C. to obtain an activated carbon electrode sheet.
[0054] The capacitive desalination system of this embodiment was powered on for capacitive deionization, and a sodium chloride aqueous solution was used as a model system to simulate brackish water with sodium chloride as the main salt component. In a sodium chloride solution with an initial concentration of 500 mg / L, the adsorption amount of the electrolyte-enhanced electrode material in the system shown in this embodiment was evaluated at different voltages, and the experimental results are as follows:
[0055] from Figure 4 The significant enhancement in the desalination capacity of the system was observed, which was mainly attributed to the addition of Figure 5 The reaction mechanism shown is as follows: the cathode chamber obtains more electrons by adsorption of activated carbon and reduction of sodium ferrocyanide. In the presence of a redox couple in a 1 mol / L sodium chloride solution, the CV curve shows obvious redox peaks near 0.12 and 0.28 V (vs Ag / AgCl), while in the absence of a redox couple, the CV has a rectangular shape (e.g. Figure 6 This situation occurs due to the presence of the cation exchange membrane, which can only capture more sodium ions to achieve charge balance. At the same time, the manganese dioxide with ammonium ion hydrogen bond pre-intercalation in the anode chamber loses more electrons by breaking the hydrogen bonds. When the electrolyte is 1 mol / L ammonium chloride, the CV curve shows obvious redox peaks near -0.08 and 0.38 V (vs Ag / AgCl), while when the electrolyte is 1 mol / L sodium chloride, the CV has a rectangular shape (as shown in Figure 2). Figure 7 As shown in Figure 2 ). Also due to the presence of the anion exchange membrane, ammonium ions cannot leave the cathode chamber, and more chloride ions are captured to achieve charge balance. Therefore, the reduction of ferrocyanide and the breaking of hydrogen bonds are considered to be the main reasons for the enhanced desalination performance observed in this system.
[0056] At 1.2V, the reduction reaction and the breaking of hydrogen bonds increased the desalination to 51.5mg / g, compared with 27.7mg / g in conventional CDI. In the discharge step, the ions released from the cathode and cathode chambers move to the intermediate salt solution to meet the electrical neutrality in the cathode and cathode chambers. In addition, Figure 8 The desalination performance diagram of 100 cycles and initial performance is shown in Figure 2. Figure 8It can be found that after the desalination system of this embodiment has undergone 100 complete ion storage / release processes at a voltage of 1.2 V, the performance remains stable, indicating that it has good cycle stability.
[0057] Example 2: The desalination advantages of α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation as the anode of the desalination system in this system
[0058] In this embodiment, the desalination performance of manganese dioxide with different structures as the anode material of the desalination system is studied. The capacitive desalination reaction system is tested for desalination at a voltage of 1.2 V. The test process is the same as that of Example 1. The specific system structure composition and the preparation method of the electrode are similar to those of Example 1. The only difference is that the manganese dioxide of the anode material is different, as shown in the following table.
[0059] Table 1 Effect of different manganese dioxide on desalination performance in this system
[0060]
[0061] It can be observed from the table that the cycle performance of the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation is superior, while the cycle retention rate of the α-phase manganese dioxide without ammonium ion hydrogen bond pre-intercalation and the δ-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation prepared by a method similar to Example 1 is relatively poor. This is because the ammonium ions in the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation form hydrogen bonds with oxygen atoms, which can act as "structural columns" to stabilize the pore structure. The special pore structure can not only promote the storage and diffusion of ammonium ions, but also help to alleviate the structural changes caused by ion insertion / extraction during discharge / charging, thereby providing high cycle performance.
[0062] Example 3 Study on the influence of different electrolyte solutions in the anode chamber on the desalination performance of the desalination system
[0063] In this embodiment, the effects of different electrolyte solutions in the anode chamber on the delay performance of the desalination system are studied and tested. The desalination reaction system is tested at a voltage of 1.2V. The test process is the same as that in Example 1. The specific structure and composition of the desalination system and the preparation method of the electrode are similar to those in Example 1. The only difference is that the electrolyte solution in the anode chamber is different, as shown in the following table.
[0064] Table 2 Effect of different electrolyte solutions in the anode chamber on desalination performance in this system
[0065]
[0066] From the desalination test results, when the salt solution in the anode chamber is ammonium chloride, the desalination performance is the highest. The manganese dioxide with an intercalated structure prepared by the present invention utilizes the breaking of hydrogen bonds in the ammonium chloride electrolyte to transfer a large amount of electrons to adsorb chloride ions, while other salt solutions cannot form hydrogen bonds with manganese dioxide, resulting in a lower desalination amount.
[0067] Example 4 Desalination performance test at different applied voltages during desalination electrolysis
[0068] This example conducted a series of experimental studies on the desalination voltage applied to the desalination system prepared in Example 1, and the specific results are as follows:
[0069] Table 3 Effect of applied voltage on desalination performance in this system
[0070]
[0071]
[0072] For specific results, see Figure 4 ,From the outflow distribution diagram in the figure, the increase of voltage leads to the amplification of the conductivity curve obtained from the outflow of the middle channel. Figure 4 It shows that the desalination amount increases from 23.0 mg / g (at a voltage of 0.4 V) to 51.5 mg / g (at a voltage of 1.2 V), which means that sufficient voltage is required to fully utilize the charge transfer caused by the reduction reaction of ferrocyanide and the breaking of hydrogen bonds.
[0073] Example 5 Comparative Example
[0074] The following groups prepared different capacitive desalination systems, as follows:
[0075] Group A: This Example 1.
[0076] Group B: HCDI system, specifically a CDI system composed of activated carbon and manganese dioxide, which is similar to the desalination system of Example 1, except that no electrolyte is used to strengthen the activated carbon electrode and the manganese dioxide electrode.
[0077] Group C: Similar to Example 1, except that the electrolyte sodium ferrocyanide was not added to the cathode chamber, but sodium chloride was added instead.
[0078] Group D: Similar to Example 1, except that the electrolyte ammonium chloride was not added to the anode chamber, and sodium chloride was added instead.
[0079] Group E: Similar to Example 1, except that no activated carbon was added to the cathode chamber, and electrolyte sodium ferrocyanide was directly added.
[0080] Group F: Similar to Example 1, except that the electrolyte concentrations in the cathode and anode chambers were both 0.001 mol / L.
[0081] Group J: Similar to Example 1, except that the electrolyte concentration in the cathode / anode compartments was 0.05 mol / L.
[0082] The above groups were subjected to desalination electrolysis tests respectively, and the test process was the same as in Example 1, wherein the results of group AB are shown in Figure 4 .
[0083] The desalination results of the CJ group are shown in the table below.
[0084] Table 4 Desalination performance of different comparative examples in this system
[0085]
[0086] From the desalination test results of this embodiment, in the proposed system, the sodium ferrocyanide solution in the cathode chamber strengthens the activated carbon electrode to construct a functional interface to synergistically adsorb more sodium ions, and the ammonium chloride solution in the anode chamber strengthens the MnO2 with intercalated structure. 2 The electrode causes hydrogen bonds to break and synergistically adsorb more chloride ions. The two complement each other, allowing the desalination performance of CDI to break through its own threshold and reach 51.5 mg / g. When the electrolyte concentration is 0.01 mol / L, the interaction between the material and the electrolyte can be maximized without causing waste of resources.
[0087] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.
Claims
1. A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte, comprising an anode chamber, a cathode chamber and a brine chamber, wherein an anion exchange membrane close to the anode chamber and a cation exchange membrane close to the cathode chamber are arranged between the anode chamber and the cathode chamber, characterized in that: The anode chamber is provided with a manganese dioxide electrode sheet and is filled with an ammonium chloride solution, and the cathode chamber is provided with an activated carbon electrode sheet and is filled with a sodium ferrocyanide solution; the concentrations of the ammonium chloride solution and the sodium ferrocyanide solution are both 0.01 mol / L; the two adjacent ion exchange membranes in the cation exchange membrane and the anion exchange membrane pair are separated by a chamber to form a brine chamber, and the brine chamber forms a closed loop using a silicone tube; the manganese dioxide electrode sheet is connected to the activated carbon electrode sheet through a wire via an external voltage, the desalination voltage is 1.2V, and the anode chamber and the cathode chamber are connected using a silicone tube to form a closed loop; The manganese dioxide electrode sheet is prepared in the following steps: S1. Preparation of manganese dioxide with ammonium ion hydrogen bond pre-intercalation S11, dissolving sodium permanganate and ammonium sulfate in deionized water to form sodium permanganate solution and ammonium sulfate solution, respectively, mixing the sodium permanganate and ammonium sulfate solutions at a molar ratio of 2:1 and stirring them magnetically to obtain a mixed solution; S12, transferring the obtained mixed solution to a reaction kettle and reacting it at 170-190° C. for 16 h, and cooling it to room temperature after the reaction is completed to obtain a suspension; S13, centrifuging and washing the suspension three times respectively, and then placing the solid product in a freeze drying oven for freeze drying to obtain α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation; The α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation has a nanorod morphology with a pore diameter of 50 nm; S2. Preparation of manganese dioxide electrode sheet The product prepared in step S1 is ground into powder, and the powder is mixed with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, and then anhydrous ethanol is added to the mixture, and stirred for 20 minutes to obtain a slurry mixture, and the slurry mixture is evenly applied on a graphite plate, and dried at 80°C to obtain a manganese dioxide electrode sheet; In step S2, the mass ratio of the α-phase manganese dioxide with ammonium ion hydrogen bond pre-intercalation layer to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone is 20:8.6:5:7.
5.
2. A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte according to claim 1, characterized in that: The activated carbon electrode sheet is prepared in the following steps: The activated carbon was ground into powder and mixed evenly with acetylene black, polyvinyl butyral and polyvinyl pyrrolidone to obtain a mixture, and then anhydrous ethanol was added to the mixture and stirred for 20 min to obtain a slurry mixture. The slurry mixture was evenly applied on a graphite plate and dried at 80 °C to obtain an activated carbon electrode sheet.
3. A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte according to claim 1, characterized in that: In step S13, the freeze-drying temperature is -60°C and the time is 12 h.
4. A capacitive deionization system capable of strengthening its electrode material with the aid of an electrolyte according to claim 1, characterized in that: In step S2, the slurry mixture is evenly applied on the graphite plate with a thickness of 0.3-0.5 mm.
5. A capacitive deionization system capable of strengthening its electrode material with the aid of electrolyte according to claim 2, characterized in that: The mass ratio of activated carbon to acetylene black, polyvinyl butyral and polyvinyl pyrrolidone is 20:8.6:5:7.
5.
6. A capacitive deionization system capable of strengthening its electrode material with the aid of electrolyte according to claim 2, characterized in that: The slurry mixture is evenly spread on the graphite plate with a thickness of 0.3-0.5 mm.