A nonionic waterborne epoxy curing agent and preparation method thereof

By reacting small molecule ketone with diethylene triamine to form diethylene triamine imine, and reacting with polyethylene glycol diglycidyl ether and hydrophobic epoxy resin, a nonionic aqueous epoxy curing agent is solved The problems of high production costs and insufficient performance in the prior art have achieved low-cost and high-performance paint film performance improvement.

CN115894865BActive Publication Date: 2024-12-03GUANGDONG HUAGUOSHAN ENVIRONMENTAL PROTECTION SCI-TEC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211644892.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-12-03
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The existing non-ionic aqueous epoxy curing agents have high production costs, which limits their wide application and is difficult to impart excellent boiling water, acid and alkali resistance and neutral salt spray resistance to paint films in the aqueous epoxy emulsion composite film. .

Method used

Diethylene triamine imine is formed by reacting small molecule ketone with diethylene triamine and reacting with polyethylene glycol diglycidyl ether and hydrophobic epoxy resin in a hydrophilic solvent to form nonionic aqueous epoxy The curing agent uses a simple preparation process and cheap raw materials to form a punctured supramolecular structure to shield acid and alkali ions and chemical media.

Benefits of technology

It realizes a non-ionic aqueous epoxy curing agent with low preparation cost and simple process, which imparts excellent boiling water, acid and alkali resistance and neutral salt spray resistance to paint films, making it suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004009405970000051
    Figure BDA0004009405970000051
Patent Text Reader

Abstract

The present invention discloses a nonionic waterborne epoxy curing agent and a preparation method thereof. The preparation method of the nonionic waterborne epoxy curing agent of the present invention comprises the following steps: 1) mixing a small molecule ketone and diethylenetriamine to react to obtain diethylenetriamine ketone imine; 2) dispersing diethylenetriamine ketone imine, polyethylene glycol diglycidyl ether and a hydrophobic epoxy resin having a diepoxy group in a hydrophilic solvent to react to obtain a hydrophilically modified diethylenetriamine ketone imine; 3) mixing the hydrophilically modified diethylenetriamine ketone imine, monoglycidyl ether and water to react to obtain a nonionic waterborne epoxy curing agent. The nonionic waterborne epoxy curing agent of the present invention is compounded with a waterborne epoxy emulsion to form a film, which can give the paint film excellent properties such as resistance to boiling water, acid and alkali, and neutral salt spray, and the preparation process is simple, the production cost is low, and it is suitable for large-scale industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy curing agents, and in particular to a non-ionic water-based epoxy curing agent and a preparation method thereof. Background Art

[0002] Epoxy resin emulsion can be used in water-based epoxy coatings, adhesives, reactive diluents, cement mortar repair materials, sizing agents for glass fibers or carbon fibers, anti-corrosion primers, etc., and its application range is becoming wider and wider. Non-ionic water-based epoxy curing agent is a commonly used curing agent for epoxy resin emulsion. It is generally made by grafting polyethylene glycol ether to provide hydrophilicity, grafting epoxy resin to provide compatibility with epoxy resin emulsion, and then self-emulsification. It has the advantages of good storage stability and excellent salt spray resistance of the paint film formed by compounding with water-based epoxy emulsion. However, although some non-ionic water-based epoxy curing agents on the market can be compounded with water-based epoxy emulsion to form a film to give the paint film excellent resistance to boiling water and chemical media, most of these curing agents need to use expensive meta-phenylenediamine (the benzene ring in the molecular structure provides excellent heat and chemical resistance, and the aliphatic primary amine provides room temperature curing performance) as a raw material, the production cost is high, and the application is greatly limited.

[0003] Therefore, it is of great significance to develop a non-ionic water-based epoxy curing agent with simple preparation process, low production cost, and the ability to form a film with water-based epoxy emulsion to give the paint film excellent resistance to boiling water, acid and alkali, and neutral salt spray.

[0004] The above statements merely provide background information related to the present invention and do not necessarily constitute prior art. Summary of the invention

[0005] The object of the present invention is to provide a nonionic waterborne epoxy curing agent and a preparation method thereof.

[0006] The technical solution adopted by the present invention is:

[0007] A method for preparing a nonionic waterborne epoxy curing agent comprises the following steps:

[0008] 1) mixing a small molecule ketone and diethylenetriamine to react to obtain diethylenetriamine ketimine;

[0009] 2) dispersing diethylenetriamine ketimine, polyethylene glycol diglycidyl ether and a hydrophobic epoxy resin having a diepoxy group in a hydrophilic solvent for reaction to obtain a hydrophilically modified diethylenetriamine ketimine;

[0010] 3) The hydrophilic modified diethylenetriamine ketimine, monoglycidyl ether and water are mixed and reacted to obtain a non-ionic waterborne epoxy curing agent.

[0011] Preferably, the small molecule ketone in step 1) is at least one of acetone, butanone and methyl isobutyl ketone.

[0012] Preferably, in step 1), the molar ratio of the small molecule ketone to diethylenetriamine is 1.8-2.0:1.

[0013] Preferably, the reaction in step 1) is carried out at 80°C to 120°C, and the reaction time is 6h to 12h.

[0014] Preferably, the specific operation of step 1) is: mixing a small molecule ketone and diethylenetriamine to react, and removing the water produced by the reaction in time during the reaction, and then performing a vacuum operation for 1h to 3h at a temperature of 100°C to 120°C and a vacuum degree of -0.1MPa to -0.06MPa (to remove excess small molecule ketones) to obtain diethylenetriamine ketone imine.

[0015] Preferably, the number average molecular weight of the polyethylene glycol diglycidyl ether in step 2) is 600 g / mol to 2200 g / mol.

[0016] Preferably, the hydrophobic epoxy resin having a diepoxy group in step 2) is at least one of epoxy resin E51, epoxy resin E44, and epoxy resin E20.

[0017] Preferably, in step 2), the molar ratio of the diethylenetriamine ketimine to the total epoxy groups in the polyethylene glycol diglycidyl ether and the hydrophobic epoxy resin having diepoxy groups is 1:1.0-1.2.

[0018] Preferably, in step 2), the mass ratio of the polyethylene glycol diglycidyl ether to the hydrophobic epoxy resin having a diepoxy group is 0.39 to 0.77:1.

[0019] Preferably, in step 2), the mass ratio of the hydrophobic epoxy resin having diepoxy groups to the hydrophilic solvent is 1:0.38-0.64.

[0020] Preferably, the hydrophilic solvent in step 2) is at least one of ethanol, isopropanol, propylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.

[0021] Preferably, the reaction in step 2) is carried out at 60°C to 90°C, and the reaction time is 2h to 4h.

[0022] Preferably, the monoglycidyl ether in step 3) is C1~C 14 At least one of alkyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether and cardanol glycidyl ether.

[0023] Preferably, the molar ratio of the epoxy groups in the diethylenetriamine ketimine in step 2) and the monoglycidyl ether in step 3) is 1:0.2-1.0.

[0024] Preferably, the molar ratio of the diethylenetriamine ketimine in step 2) to the water in step 3) is 1:3.0-5.0.

[0025] Preferably, the reaction in step 3) is carried out at 60°C to 90°C, and the reaction time is 2h to 5h.

[0026] A nonionic waterborne epoxy curing agent is prepared by the above preparation method.

[0027] The beneficial effects of the present invention are as follows: the nonionic waterborne epoxy curing agent of the present invention is compounded with the waterborne epoxy emulsion to form a film, which can give the paint film excellent properties such as resistance to boiling water, acid and alkali, and neutral salt spray, and the preparation process is simple and the production cost is low, and it is suitable for large-scale industrial application.

[0028] Specifically:

[0029] 1) The present invention is based on diethylenetriamine ketimine to prepare a non-ionic waterborne epoxy curing agent (ketimine method), which is cross-linked with epoxy resin to form a regular branched supramolecular structure. The supramolecular branched structure can effectively shield acid and alkali ions and other chemical media, and ultimately can give the paint film excellent properties such as resistance to boiling water, acid and alkali, and neutral salt spray;

[0030] 2) The raw materials of the nonionic waterborne epoxy curing agent of the present invention are cheap and readily available, the preparation cost is low, the process is simple, and it is suitable for large-scale industrial production. DETAILED DESCRIPTION

[0031] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0032] Embodiment 1:

[0033] A nonionic waterborne epoxy curing agent, the preparation method of which comprises the following steps:

[0034] 1) Acetone and diethylenetriamine are mixed in a molar ratio of 1.8:1, reacted at 80° C. for 10 h, and water produced by the reaction is removed in time during the reaction, and then vacuumed for 2 h at a temperature of 100° C. and a vacuum degree of -0.06 MPa (to remove excess acetone) to obtain diethylenetriamine ketimine;

[0035] 2) 175 g of diethylenetriamine ketimine, 120 g of polyethylene glycol diglycidyl ether with a number average molecular weight of 600 g / mol, and 156 g of epoxy resin E51 were dispersed in 60 g of propylene glycol methyl ether (the molar ratio of diethylenetriamine ketimine to the total epoxy groups in polyethylene glycol diglycidyl ether and epoxy resin E51 was 1:1.2), and reacted at 60° C. for 4 h to obtain hydrophilically modified diethylenetriamine ketimine;

[0036] 3) Mix hydrophilically modified diethylenetriamine ketimine, 36 g of phenyl glycidyl ether, 44 g of benzyl glycidyl ether and 54 g of water (the molar ratio of diethylenetriamine ketimine to the epoxy groups in phenyl glycidyl ether and benzyl glycidyl ether is 1:0.4, and the molar ratio of diethylenetriamine ketimine to water is 1:3.0), and react at 70°C for 5 hours to obtain a non-ionic waterborne epoxy curing agent.

[0037] Embodiment 2:

[0038] A nonionic waterborne epoxy curing agent, the preparation method of which comprises the following steps:

[0039] 1) butanone and diethylenetriamine were mixed in a molar ratio of 1.92:1, reacted at 100° C. for 6 h, and the water produced by the reaction was removed in time during the reaction, and then vacuumed for 1 h at a temperature of 110° C. and a vacuum degree of -0.07 MPa to obtain diethylenetriamine ketimine;

[0040] 2) 207 g of diethylenetriamine ketimine, 120 g of polyethylene glycol diglycidyl ether having a number average molecular weight of 1200 g / mol, and 205 g of epoxy resin E44 were dispersed in 42.5 g of isopropanol and 60 g of ethylene glycol butyl ether (the molar ratio of diethylenetriamine ketimine to the total epoxy groups in polyethylene glycol diglycidyl ether and epoxy resin E44 was 1:1.1), and reacted at 70° C. for 3 h to obtain hydrophilically modified diethylenetriamine ketimine;

[0041] 3) Mix hydrophilic modified diethylenetriamine ketimine, 56 g of carbon dodecyl glycidyl ether, 44 g of benzyl glycidyl ether, 75 g of cardanol glycidyl ether and 63 g of water (the molar ratio of diethylenetriamine ketimine to the epoxy groups in carbon dodecyl glycidyl ether, benzyl glycidyl ether and cardanol glycidyl ether is 1:0.6, and the molar ratio of diethylenetriamine ketimine to water is 1:3.5), react at 80°C for 3h to obtain a non-ionic waterborne epoxy curing agent.

[0042] Embodiment 3:

[0043] A nonionic waterborne epoxy curing agent, the preparation method of which comprises the following steps:

[0044] 1) Methyl isobutyl ketone and diethylenetriamine were mixed in a molar ratio of 2.0:1, reacted at 120° C. for 12 hours, and the water produced by the reaction was removed in time during the reaction, and then vacuumed for 3 hours at a temperature of 120° C. and a vacuum degree of -0.09 MPa to obtain diethylenetriamine ketimine;

[0045] 2) 267 g of diethylenetriamine ketimine, 100 g of polyethylene glycol diglycidyl ether having a number average molecular weight of 2200 g / mol, 157 g of epoxy resin E51 and 100 g of epoxy resin E20 were dispersed in 50 g of ethanol and 50 g of propylene glycol methyl ether acetate (the molar ratio of diethylenetriamine ketimine to the total epoxy groups in polyethylene glycol diglycidyl ether, epoxy resin E51 and epoxy resin E20 was 1:1.0), and reacted at 80° C. for 3 h to obtain hydrophilically modified diethylenetriamine ketimine;

[0046] 3) Mix the hydrophilically modified diethylenetriamine ketimine, 160 g of butyl glycidyl ether and 72 g of water (the molar ratio of the epoxy groups in diethylenetriamine ketimine and butyl glycidyl ether is 1:1.0, and the molar ratio of diethylenetriamine ketimine and water is 1:4.0), and react at 90° C. for 2 h to obtain a non-ionic waterborne epoxy curing agent.

[0047] Embodiment 4:

[0048] A nonionic waterborne epoxy curing agent, the preparation method of which comprises the following steps:

[0049] 1) butanone and diethylenetriamine were mixed in a molar ratio of 1.88:1, reacted at 95° C. for 10 h, and the water produced by the reaction was removed in time during the reaction, and then vacuumed for 1.5 h at a temperature of 105° C. and a vacuum degree of -0.08 MPa to obtain diethylenetriamine ketimine;

[0050] 2) 204 g of diethylenetriamine ketimine, 96 g of polyethylene glycol diglycidyl ether with a number average molecular weight of 1200 g / mol, 98 g of epoxy resin E51 and 90 g of epoxy resin E44 were dispersed in 120 g of propylene glycol methyl ether (the molar ratio of diethylenetriamine ketimine to the total epoxy groups in polyethylene glycol diglycidyl ether, epoxy resin E51 and epoxy resin E44 was 1:1.15), and reacted at 75° C. for 2.5 h to obtain hydrophilically modified diethylenetriamine ketimine;

[0051] 3) Mix the hydrophilically modified diethylenetriamine ketimine, 80 g of cardanol glycidyl ether and 90 g of water (the molar ratio of the epoxy groups in diethylenetriamine ketimine and cardanol glycidyl ether is 1:0.2, and the molar ratio of diethylenetriamine ketimine and water is 1:5.0), and react at 60° C. for 4 h to obtain a non-ionic waterborne epoxy curing agent.

[0052] Comparative Example 1:

[0053] Huntsman's waterborne epoxy curing agent 3986.

[0054] Comparative Example 2:

[0055] Water-based epoxy curing agent GZ12 from Guangdong Huaguoshan Environmental Protection Technology Co., Ltd.

[0056] Performance Test:

[0057] The performance of the waterborne epoxy curing agent of Examples 1 to 4 and Comparative Examples 1 to 2 was tested, and the test results are shown in the following table:

[0058] Table 1 Performance test results of waterborne epoxy curing agents of Examples 1 to 4 and Comparative Examples 1 to 2

[0059]

[0060] Note:

[0061] Solid content: Tested in accordance with "GB 1725-1979 Determination of solid content of coatings";

[0062] Amine hydrogen equivalent: Tested in accordance with "GB / T 7383-2020 Determination of hydroxyl value of non-ionic surfactants";

[0063] Viscosity: Tested in accordance with "GB / T 22235-2008 Determination of Liquid Viscosity";

[0064] Adhesion: Tested in accordance with "GB / T 9286-2021 Paint and varnish cross-cut test";

[0065] Boiling water resistance: Tested in accordance with "GB / T 4893.1-2005 Furniture surface resistance to cold liquid";

[0066] Resistance to 5% sulfuric acid: Tested in accordance with "GB / T 4893.1-2005 Furniture surface cold liquid resistance test method";

[0067] Resistance to 5% sodium hydroxide: Tested in accordance with "GB / T 4893.1-2005 Furniture surface cold liquid resistance test method";

[0068] Hardness: Test according to "ASTM D3363-2000 Pencil Test for Determination of Paint Film Hardness";

[0069] Neutral salt spray resistance time: Tested in accordance with "GB / T 1771-1991 Determination of neutral salt spray resistance of paints and varnishes".

[0070] Preparation of paint film: The epoxy emulsion EP361 of Guangdong Huaguoshan Environmental Protection Technology Co., Ltd. was mixed evenly with the water-based epoxy curing agent of Examples 1 to 4 and Comparative Examples 1 to 2 according to the epoxy value and active hydrogen equivalent ratio of 1:0.8, and then sprayed on the sandblasted steel plate and cured at room temperature for 168 hours.

[0071] It can be seen from Table 1 that the various properties of the nonionic waterborne epoxy curing agent of the present invention are comparable to those of Huntsman's waterborne epoxy curing agent. 3986, and can completely replace expensive imported products, thereby effectively reducing costs. It is significantly superior to the water-based epoxy curing agent GZ12 of Guangdong Huaguoshan Environmental Protection Technology Co., Ltd. in terms of paint film resistance to boiling water, acid and alkali resistance, and neutral salt spray resistance.

[0072] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a nonionic waterborne epoxy curing agent, characterized in that: The following steps are involved: 1) Mix a small molecule ketone and diethylenetriamine to react to obtain diethylenetriamine ketimine; 2) dispersing diethylenetriamine ketimine, polyethylene glycol diglycidyl ether and a hydrophobic epoxy resin having a diepoxy group in a hydrophilic solvent for reaction to obtain a hydrophilically modified diethylenetriamine ketimine; 3) mixing hydrophilic modified diethylenetriamine ketimine, monoglycidyl ether and water to react, thereby obtaining a non-ionic waterborne epoxy curing agent; Step 1) the small molecule ketone is at least one of acetone, butanone and methyl isobutyl ketone; Step 2) the number average molecular weight of the polyethylene glycol diglycidyl ether is 600 g / mol to 2200 g / mol; Step 2) the hydrophobic epoxy resin having a diepoxy group is at least one of epoxy resin E51, epoxy resin E44, and epoxy resin E20; Step 3) The monoglycidyl ether is C1~C 14 At least one of alkyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, and cardanol glycidyl ether; Step 1) The molar ratio of the small molecule ketone to diethylenetriamine is 1.8 to 2.0:1; Step 2) the molar ratio of the diethylenetriamine ketimine to the total epoxy groups in the polyethylene glycol diglycidyl ether and the hydrophobic epoxy resin having diepoxy groups is 1:1.0-1.2; Step 2) the mass ratio of the polyethylene glycol diglycidyl ether to the hydrophobic epoxy resin having a diepoxy group is 0.39 to 0.77:1; The molar ratio of the epoxy groups in the diethylenetriamine ketimine in step 2) and the monoglycidyl ether in step 3) is 1:0.2-1.

0.

2. The method for preparing the nonionic waterborne epoxy curing agent according to claim 1, characterized in that: Step 1) The reaction is carried out at 80°C to 120°C for 6h to 12h.

3. The method for preparing the nonionic waterborne epoxy curing agent according to claim 1, characterized in that: Step 2) The hydrophilic solvent is at least one of ethanol, isopropanol, propylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol methyl ether acetate.

4. The method for preparing the nonionic waterborne epoxy curing agent according to claim 1, characterized in that: Step 2) The reaction is carried out at 60°C to 90°C for 2h to 4h.

5. The method for preparing the nonionic waterborne epoxy curing agent according to claim 1, characterized in that: The molar ratio of the diethylenetriamine ketimine in step 2) to the water in step 3) is 1:3.0-5.

0.

6. The method for preparing the nonionic waterborne epoxy curing agent according to claim 1 or 5, characterized in that: Step 3) The reaction is carried out at 60°C to 90°C for 2h to 5h.

7. A nonionic waterborne epoxy curing agent, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.