A high-precision graphic coating organic silicon protective film and preparation method thereof
Through a one-step process, high-precision graphic coated silicone protective film is constructed, which solves the problem of the production of electronic product screen packaging protective films that consume a lot of labor time and large material losses, and realizes high-precision graphic coating and de-plasticization, simplifying The die-cutting process improves environmental protection performance.
Patent Information
- Application Number
- CN202211352787.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-31
AI Technical Summary
The preparation process of existing electronic product screen packaging protective films consumes a lot of labor time and has large material losses, and does not conform to the trend of "deplastication" and "low-carbon" environmental protection, especially the substrate and glueless support films are plasticized materials.
A one-step process is used to build a high-precision graphic coated silicone protective film, and a pattern printing with glue/free areas is achieved through silk-printing and gravure printing, reducing double-sided adhesive coating and composite processes, using paper substrates and passing back Wet treatment improves the flatness of the rubber surface and reduces carbon emissions.
High-precision pattern coating is realized, the edge linearity tolerance of the silicone pressure-sensitive adhesive layer is less than 1mm, and the gloss of the glue surface is 65-100, simplified die cutting process, save raw materials, and realize de-plasticization of electronic product screen protector film , improve process efficiency and environmental performance.
Smart Images

Figure CN115895470B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of protective films, in particular to a high-precision graphic coated organic silicon protective film and a preparation method thereof. Background Art
[0002] Protective film is a flat material with certain self-adhesive or adsorbent properties, used to protect the surface of high-value precision products. Protective film is widely used in the processing, production, storage and transportation of electronic products. Consumers are most exposed to the protective film of the screen packaging of electronic products. The adhesive part is attached to the screen of the electronic product to protect the screen before the consumer opens the box. The factory packaging of the screen has a protruding non-adhesive handle area, and consumers can easily peel off the protective film from the handle and start using the electronic product.
[0003] The protective film has an adhesive part and a non-adhesive part, and is usually prepared by a die-cutting composite process: first, a full-width double-sided adhesive product is prepared ( Figure 1-1 01), a weakly sticky silicone pressure-sensitive adhesive is coated on one side of the film substrate, and a strong sticky polyacrylate adhesive is coated on the other side. After die-cutting into the shape of the screen, the strong sticky side of the double-sided adhesive is connected to the adhesive-free support film ( Figure 1-1 02) Compounding, die-cutting again to cut off the composite area as a whole and enlarge the die-cut edge to add a non-glue handle, so as to obtain a screen protective film product with a non-glue handle.
[0004] Obviously, the energy consumption and material loss of the above-mentioned method of preparing adhesive / non-adhesive graphic protective film products by die-cutting composite double-sided adhesive and non-adhesive support film are relatively large, which is not in line with the environmental protection trend of electronic product packaging materials pursuing "plastic removal" and "low carbon". Summary of the invention
[0005] The first purpose of the invention of this application is to provide a high-precision graphic coated silicone protective film and a preparation method thereof, which constructs a graphic adhesive / non-adhesive area through a one-step process, eliminating the double-sided adhesive coating and composite process, so as to solve the problem of large amount of raw materials used in the factory packaging protective film of electronic product screens and complex die-cutting process resulting in more work time in the background technology.
[0006] The second purpose of the invention of this application is to provide a high-precision graphic coated paper substrate silicone protective film and a preparation method thereof, so as to reduce the use of non-renewable "plastic" raw materials and reduce total carbon emissions, so as to solve the problem that the substrate and the glue-free supporting film of the factory packaging protective film of the electronic product screen in the background technology are plasticized materials, which do not conform to the "plastic removal" and "low carbon" environmental protection trends.
[0007] The above-mentioned invention objective of the present application is achieved through the following technical solutions:
[0008] A graphic glue / non-glue area is constructed through a one-step process, eliminating the need for double-sided adhesive coating and composite process. In order to achieve high-precision graphic glue coating technology, it is necessary to refer to silk screen printing and gravure printing processes. The two processes are respectively graphic plate-making through the micro-carving holes of the silk screen grid and the screen roller, and can achieve high-dimensional precision graphic printing effects by accurately transferring the pixel matrix of the screen / roller plate.
[0009] The accuracy of the graphics is related to the mesh count of the screen / screen roller. The higher the mesh count, the denser the pixel matrix, the smaller the single pixel, and the smaller the straightness tolerance of the jagged edge formed by the fusion of the pixel matrix at the edge of the print ( Figure 2-2 04), that is, the higher the graphics accuracy, the clearer the edges ( Figure 2-2 03). At the same time, the higher the mesh count of the screen / roller plate, the smaller the amount of ink / glue transferred and the thinner the ink / glue layer.
[0010] For protective films, the thickness and flatness of the adhesive layer are crucial to product application. The adhesive layer needs to reach a certain thickness to have enough deformation space to fill the surface undulations of the adhered object and achieve effective adsorption and bonding. For screen protective films, the adhesive thickness is usually set at 5 to 30 μm; at the same time, the adhesive surface must be flat enough to ensure complete adsorption of large-area bonding and avoid bonding bubbles. The flatness of the adhesive surface can be evaluated by the glossiness of the adhesive surface. The glossiness Gu value (60°) of the adhesive surface of the screen protective film is usually controlled above 65.
[0011] The technical solution of the present invention is specifically: a high-precision graphic coated silicone protective film, which includes a silicone pressure-sensitive adhesive layer and a printing substrate, the silicone pressure-sensitive adhesive layer is graphic printed on the printing substrate, and the printing substrate is divided into a corresponding screen part and a handle part connected to each other; the silicone pressure-sensitive adhesive layer covers the corresponding screen part of the printing substrate, and the handle part of the printing substrate is a non-adhesive area; the edge area straightness tolerance of the silicone pressure-sensitive adhesive layer is less than 1mm.
[0012] Furthermore, the total mass proportion of the diluent in the pressure-sensitive adhesive of the organic silicone pressure-sensitive adhesive layer does not exceed 30%, and the viscosity of the pressure-sensitive adhesive is between 500-5000 cps.
[0013] Furthermore, the composition ratio of the pressure-sensitive adhesive of the organic silicone pressure-sensitive adhesive layer is as follows in parts by weight:
[0014] Silicone oil 50-90 parts; high viscosity silicone glue 10-50 parts; diluent 0-30 parts; cross-linking agent 1-3 parts; inhibitor 0.05-0.2 parts; catalyst 0.5-2 parts;
[0015] The viscosity of the silicone oil is 500 cps to 10000 cps, preferably, the viscosity of the silicone oil is 500 to 2000 cps. The molar fraction of vinyl is 0.10% to 0.60%.
[0016] The high-viscosity silicone glue is a silicone rubber solution modified by MQ resin, with a solid content of 65-80%, and the remaining components are diluents. The viscosity of the high-viscosity silicone glue is 800-50000cps, and preferably the viscosity of the high-viscosity silicone glue is 800-4000cps.
[0017] The diluent is a mixture of one or more of toluene, ethyl acetate, butyl acetate, heptane, isophorone, solvent oil or petroleum ether.
[0018] The cross-linking agent is silicone oil containing active silicon hydrogen (-SiH) groups.
[0019] The inhibitor is a combination of one or more of alkynol compounds, maleic acid and its derivatives, and fumaric acid and its derivatives.
[0020] The catalyst is a platinum catalyst, and the platinum content is 2000-8000ppm.
[0021] Furthermore, the surface of the organic silicone pressure-sensitive adhesive layer is smooth and flat, and the glossiness Gu value of the adhesive surface is 65-100, and the Gu value is measured at 60°.
[0022] Furthermore, the printing substrate is a smooth, flat, liquid-impermeable polymer film, which may be a PET film, a PI film, a PP film or other liquid-impermeable polymer film.
[0023] A method for preparing a high-precision patterned coated organic silicon protective film comprises the following steps:
[0024] (1) weighing silicone oil, high-viscosity silicone glue, diluent, cross-linking agent, inhibitor, and catalyst according to the formula amount, and mixing them evenly to obtain a pressure-sensitive adhesive glue;
[0025] (2) Using a screen printing process, the pressure-sensitive adhesive is graphically transferred to the printing substrate through a custom-patterned screen;
[0026] (3) The pressure-sensitive adhesive transferred to the printing substrate undergoes a 20-600 s room temperature leveling process to allow the pixel matrix of the pressure-sensitive adhesive to be fully integrated and leveled;
[0027] (4) The patterned pressure-sensitive adhesive that has undergone the leveling process enters an oven, where it undergoes a high temperature process of 90 to 160° C. to volatilize the solvent and simultaneously undergo a curing reaction to form a silicone pressure-sensitive adhesive layer;
[0028] (5) A release layer is bonded to the adhesive surface of the silicone pressure-sensitive adhesive layer to obtain a high-precision patterned coated silicone protective film.
[0029] Furthermore, step (2) is: graphically transferring the pressure-sensitive adhesive to the printing substrate through a gravure plate with a customized pattern by gravure printing process.
[0030] The above scheme can be used to prepare a high-precision graphic coated silicone protective film with a thickness of 5-20μm; the edge area of the silicone pressure-sensitive adhesive layer is clear, and the straightness tolerance is less than 1mm; the adhesive surface is flat and smooth, and the glossiness of the adhesive surface is between 65-100. The protective film product with a non-adhesive handle can be produced by one-step die-cutting. The protective film has excellent adsorption and bonding properties and can be bonded to the protected material over a large area without generating bonding bubbles.
[0031] The second object of the invention is achieved by the following technical solutions:
[0032] In order to achieve the goal of completely removing plastic from mobile phone screen protective films, there are two technical difficulties that need to be overcome: first, the protective film needs a non-glue handle area for consumers to hold and remove the protective film, and abandoning the paper / double-sided tape composite structure requires graphical coating on the paper surface; second, the surface of the paper itself is not flat and smooth and has a porous structure. The glue is easy to penetrate this structure, which is not conducive to forming a flat and smooth glue surface and thus affects the application effect of the protective film.
[0033] For the first difficulty, the first invention objective of this application has been solved. For the second difficulty, on the basis of high-precision graphic coating, the pressure-sensitive adhesive needs to be fully leveled on the paper substrate to compensate for the impact of the roughness of the paper substrate itself on the flatness of the adhesive surface and to minimize the penetration of the glue into the paper to avoid the reduction of the effective glue thickness affecting the bonding effect.
[0034] For protective films, the thickness and flatness of the adhesive layer are crucial to product application. The adhesive layer needs to reach a certain thickness to have enough deformation space to fill the undulations on the surface of the object to be attached and achieve effective adsorption and bonding. For screen protective films, the adhesive thickness is usually set at 5-30μm; at the same time, the adhesive surface must be flat enough to ensure complete adsorption of large-area bonding and avoid bonding bubbles. The flatness of the adhesive surface can be evaluated by the glossiness of the adhesive surface. The glossiness Gu value (60°) of the adhesive surface of the screen protective film is usually controlled above 65. On the paper substrate, sufficient leveling requires reducing the viscosity of the glue and increasing the leveling time, but accordingly, the above operations will increase the penetration of the glue into the paper and reduce the effective glue thickness. It is necessary to control the physical properties of the pressure-sensitive adhesive and the graphic coating process settings particularly accurately to achieve high-precision graphic coating on the paper while ensuring the effective glue thickness and the glossiness of the glue surface to obtain a good bonding effect.
[0035] The technical solution of the present invention is specifically: a high-precision graphic coated silicone protective film, which includes a silicone pressure-sensitive adhesive layer and a printing substrate, the silicone pressure-sensitive adhesive layer is graphic printed on the printing substrate, and the printing substrate is divided into a corresponding screen part and a handle part connected to each other; the silicone pressure-sensitive adhesive layer covers the corresponding screen part of the printing substrate, and the handle part of the printing substrate is a glue-free area; the straightness tolerance of the edge area of the silicone pressure-sensitive adhesive layer is less than 1mm; the printing substrate is a paper substrate.
[0036] The paper substrate is one of coated paper, kraft paper or glassine paper.
[0037] The paper substrate needs to be rehumidified after the oven drying and curing process, and the difference in moisture content of the paper before and after drying is less than 3%.
[0038] Furthermore, the total mass of the diluent in the pressure-sensitive adhesive of the organic silicone pressure-sensitive adhesive layer accounts for 5-18%, and the viscosity is between 800-3000 cps.
[0039] Furthermore, the composition ratio of the pressure-sensitive adhesive of the organic silicone pressure-sensitive adhesive layer is as follows in parts by weight:
[0040] 70-90 parts of silicone oil; 10-30 parts of high-viscosity silicone glue; 0-15 parts of diluent; 1-3 parts of cross-linking agent; 0.05-0.2 parts of inhibitor; 0.5-2 parts of catalyst.
[0041] Furthermore, the viscosity of the silicone oil is 500 cps to 8000 cps, preferably, the viscosity of the silicone oil is 500 to 1500 cps. The molar fraction of vinyl is 0.10% to 0.60%.
[0042] Furthermore, the high-viscosity silicone glue is a silicone rubber solution modified by MQ resin, with a solid content of 70-90%, and the remaining components are diluents. The viscosity of the high-viscosity silicone glue is 800-50000cps, and preferably the viscosity of the high-viscosity silicone glue is 800-3000cps.
[0043] Furthermore, the diluent is a mixture of one or more of toluene, ethyl acetate, butyl acetate, heptane, isophorone, solvent oil or petroleum ether.
[0044] Furthermore, the cross-linking agent is silicone oil containing active silicon hydrogen (-SiH) groups.
[0045] Furthermore, the inhibitor is a combination of one or more of alkynol compounds, maleic acid and its derivatives, and fumaric acid and its derivatives.
[0046] Furthermore, the catalyst is a platinum catalyst with a platinum content of 2000 to 8000 ppm.
[0047] A method for preparing a high-precision patterned coated organic silicon protective film comprises the following steps:
[0048] (1) weighing silicone oil, high-viscosity silicone glue, diluent, cross-linking agent, inhibitor, and catalyst according to the formula amount, and mixing them evenly to obtain a pressure-sensitive adhesive glue;
[0049] (2) By screen printing, the pressure-sensitive adhesive is graphically transferred to the printing paper substrate through a custom-patterned screen;
[0050] (3) The pressure-sensitive adhesive transferred to the printing paper substrate undergoes a 30-300 s room temperature leveling process to allow the pixel matrix of the pressure-sensitive adhesive to be fully integrated and leveled;
[0051] (4) The patterned pressure-sensitive adhesive that has undergone the leveling process enters an oven, where it undergoes a high temperature process of 90 to 160° C. to volatilize the solvent and simultaneously undergo a curing reaction to form a silicone pressure-sensitive adhesive layer;
[0052] (5) rewetting the printing paper substrate;
[0053] (6) A release layer is bonded to the adhesive surface of the silicone pressure-sensitive adhesive layer to obtain a high-precision patterned coated silicone protective film.
[0054] The above scheme can be used to prepare a high-precision graphic coated silicone protective film on a paper substrate, with a thickness of 5-20μm; the edge area of the silicone pressure-sensitive adhesive layer is clear, with a straightness tolerance of <1mm; the adhesive surface is flat and smooth, with a glossiness of 65-100. A protective film product with a non-adhesive handle can be produced in one step of die-cutting. The protective film has excellent adsorption and bonding properties and can be bonded to a large area of the protected material without generating bonding bubbles.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] 1. In the prior art, the screen part of the protective film for the factory packaging of electronic product screens includes a non-adhesive support film, a highly viscous polyacrylate adhesive, a substrate, and a silicone pressure-sensitive adhesive. The structure of the silicone protective film in this application is a printing substrate and a silicone pressure-sensitive adhesive layer, which reduces the use of highly viscous polyacrylate adhesives and substrates and saves raw material costs.
[0057] 2. By graphically coating the silicone pressure-sensitive adhesive on the printing substrate, the electronic product screen factory packaging protective film with handles but without adhesive can be die-cut in one step, which simplifies the die-cutting process and improves the process efficiency.
[0058] 3. By optimizing and matching the physical properties of the glue with the process parameters, the triple characteristics of high graphic dimensional accuracy, thick coating, and smooth adhesive surface of the pressure-sensitive adhesive layer are achieved, realizing a technical solution that cannot be achieved by conventional processes; the straightness tolerance of the edge area of the silicone pressure-sensitive adhesive is achieved to be less than 1mm; at the same time, the surface of the silicone pressure-sensitive adhesive layer is smooth and flat, and the glossiness Gu value of the adhesive surface is measured at 60°, and the Gu value is between 65-100.
[0059] 4. The printing substrate in this application can be a paper substrate. Compared with the prior art, a plasticized substrate and a non-adhesive support film are no longer used, and the silicone protective film is completely deplasticized;
[0060] 5. When the printing substrate is a paper substrate, the defects of the paper substrate itself that it is not smooth and has a porous structure, which is easy to penetrate and is not conducive to forming a smooth adhesive surface are overcome by optimizing the matching of the physical properties of the glue and the process parameters; after the pressure-sensitive adhesive layer is baked and cured, the paper substrate is rewetted to prevent the baked paper substrate from breaking or creasing due to moisture absorption. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 It is a schematic diagram of the structure of the protective film prepared by the die-cutting composite process in the background technology;
[0062] Figure 2 A schematic diagram of the overall result of the protective film of the present application and an enlarged view of the edge area of the silicone pressure-sensitive adhesive layer;
[0063] In the figure: 101, full-width double-sided adhesive coating; 102, adhesive-free support film; 201, protective film covering the silicone pressure-sensitive adhesive layer; 202, handle portion; 203, edge area of the silicone pressure-sensitive adhesive layer; 204, straightness tolerance of the edge area. DETAILED DESCRIPTION
[0064] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] Example 1
[0066] 70 parts of silicone oil (viscosity of 2000cps, vinyl content of 0.35%), 30 parts of high viscosity silicone glue (solid content of 65%, viscosity of 4000cps), 15 parts of toluene as a diluent, 1.5 parts of a crosslinking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring, and the mixture was stirred and mixed to obtain a pressure-sensitive adhesive with a solid content of 74.5% and a viscosity of 1900cps. The obtained glue was graphically coated on a PET film by a silk screen printing process using a 120 mesh screen printing screen, leveled at room temperature for 400s, and then placed in an oven for drying and curing. The highest point of the oven temperature was set to 150°C to ensure effective crosslinking and curing before bonding the release layer material, thereby obtaining a graphically coated high-performance paper substrate silicone protective film.
[0067] The obtained protective film has a dry adhesive thickness of 14 μm, a pattern edge straightness tolerance of 0.45 mm, and an adhesive surface glossiness Gu value (60°) of 81.5.
[0068] Example 2
[0069] 80 parts of silicone oil (viscosity of 2000cps, vinyl content of 0.35%), 20 parts of high viscosity silicone glue (solid content of 80%, viscosity of 6000cps), 20 parts of toluene as a diluent, 1.4 parts of a crosslinking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed evenly to obtain a pressure-sensitive adhesive with a solid content of 81.5% and a viscosity of 1700cps. The obtained glue was graphically coated on a PET film by a silk screen printing process using a 120 mesh screen printing screen, leveled at room temperature for 300s, and then placed in an oven for drying and curing. The highest point of the oven temperature was set to 150°C to ensure effective crosslinking and curing before bonding the release layer material, thereby obtaining a graphically coated high-performance paper substrate silicone protective film.
[0070] The obtained protective film has a dry adhesive thickness of 17 μm, a pattern edge straightness tolerance of 0.35 mm, and an adhesive surface glossiness Gu value (60°) of 79.7.
[0071] Example 3
[0072] 70 parts of silicone oil (viscosity of 2000cps, vinyl content of 0.35%), 30 parts of high viscosity silicone glue (solid content of 65%, viscosity of 4000cps), 15 parts of toluene as a diluent, 1.5 parts of a crosslinking agent (syl-off SL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed evenly to obtain a pressure-sensitive adhesive with a solid content of 74.5% and a viscosity of 1900cps. The obtained glue was graphically coated on a PET film by a silk screen printing process using a 120 mesh screen printing screen, leveled at room temperature for 400s, and then placed in an oven for drying and curing. The highest point of the oven temperature was set to 150°C to ensure effective crosslinking and curing before bonding the release layer material, thereby obtaining a graphically coated high-performance paper substrate silicone protective film.
[0073] The obtained protective film has a dry adhesive thickness of 9 μm, a pattern edge straightness tolerance of 0.25 mm, and an adhesive surface glossiness Gu value (60°) of 83.5.
[0074] Example 4
[0075] 70 parts of silicone oil (viscosity of 2000cps, vinyl content of 0.35%), 30 parts of high viscosity silicone glue (solid content of 65%, viscosity of 4000cps), 15 parts of toluene as a diluent, 1.5 parts of a crosslinking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), 1.5 parts of a catalyst (syl-off 4000; Dow Corning) were added under stirring, and the mixture was stirred and mixed to obtain a pressure-sensitive adhesive with a solid content of 74.5% and a viscosity of 1900cps. The obtained glue was graphically coated on a PET film by a gravure printing process using an 80-mesh gravure screen roll, leveled at room temperature for 500s, and then placed in an oven for drying and curing. The highest point of the oven temperature was set to 150°C to ensure effective crosslinking and curing before bonding the release layer material, thereby obtaining a graphically coated high-performance paper substrate silicone protective film.
[0076] The obtained protective film has a dry adhesive thickness of 13 μm, a pattern edge straightness tolerance of 0.49 mm, and an adhesive surface glossiness Gu value (60°) of 80.4.
[0077] Example 5
[0078] 80 parts of silicone oil (viscosity of 1800cps, vinyl content of 0.35%), 20 parts of high-viscosity silicone glue (solid content of 75%, viscosity of 3500cps), 12 parts of toluene as a diluent, 1.5 parts of a cross-linking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), and 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed to obtain a pressure-sensitive adhesive with a solid content of 85.2% and a glue viscosity of 1800cps. The obtained glue is graphically coated on coated paper with a moisture content of 7.5% through a silk-screen printing process using a 120-mesh screen, leveled for 180 seconds at room temperature, and then placed in an oven for drying and curing. The highest point of the oven temperature is set at 130°C to ensure effective cross-linking and curing. The paper is then rewetted to return the moisture content to 7.3%, and then compounded with a release layer material to obtain a graphically coated high-performance paper substrate silicone protective film.
[0079] The obtained protective film has a dry adhesive thickness of 12 μm, a pattern edge straightness tolerance of 0.37 mm, and an adhesive surface glossiness Gu value (60°) of 70.1.
[0080] Example 6
[0081] 80 parts of silicone oil (viscosity of 1800cps, vinyl content of 0.35%), 20 parts of high-viscosity silicone glue (solid content of 75%, viscosity of 3500cps), 17 parts of toluene as a diluent, 1.5 parts of a cross-linking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), and 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed to obtain a pressure-sensitive adhesive with a solid content of 85.2% and a glue viscosity of 1800cps. The obtained glue is graphically coated on coated paper with a moisture content of 7.5% through a silk-screen printing process using a 200-mesh screen, leveled for 80 seconds at room temperature, and then placed in an oven for drying and curing. The highest point of the oven temperature is set to 130°C to ensure effective cross-linking and curing. The paper is then rewetted to return the moisture content to 7.3%, and then compounded with a release layer material to obtain a graphically coated high-performance paper substrate silicone protective film.
[0082] The obtained protective film has a dry adhesive thickness of 8 μm, a pattern edge straightness tolerance of 0.26 mm, and an adhesive surface glossiness Gu value (60°) of 69.4.
[0083] Example 7
[0084] 80 parts of silicone oil (viscosity of 1800 cps, vinyl content of 0.35%), 20 parts of high-viscosity silicone glue (solid content of 80%, viscosity of 5500 cps), 8 parts of toluene as a diluent, 1.5 parts of a cross-linking agent (syl-off SL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), and 1.5 parts of a catalyst (syl-off 4000; Dow Corning) were added under stirring and mixed to obtain a pressure-sensitive adhesive with a solid content of 89.6% and a glue viscosity of 2200 cps. The obtained glue is graphically coated on coated paper with a moisture content of 7.5% through a silk-screen printing process using a 120-mesh screen, leveled for 180 seconds at room temperature, and then placed in an oven for drying and curing. The highest point of the oven temperature is set at 130°C to ensure effective cross-linking and curing. The paper is then rewetted to return the moisture content to 7.4%, and then compounded with a release layer material to obtain a graphically coated high-performance paper substrate silicone protective film.
[0085] The obtained protective film has a dry adhesive thickness of 14 μm, a pattern edge straightness tolerance of 0.33 mm, and an adhesive surface glossiness Gu value (60°) of 68.9.
[0086] Example 8
[0087] 80 parts of silicone oil (viscosity of 1800cps, vinyl content of 0.35%), 20 parts of high-viscosity silicone glue (solid content of 75%, viscosity of 3500cps), 17 parts of toluene as a diluent, 1.5 parts of a cross-linking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), and 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed to obtain a pressure-sensitive adhesive with a solid content of 81.5% and a glue viscosity of 1200cps. The obtained glue is graphically coated on coated paper with a moisture content of 7.5% through a silk-screen printing process using a 120-mesh screen, leveled for 180 seconds at room temperature, and then placed in an oven for drying and curing. The highest point of the oven temperature is set at 130°C to ensure effective cross-linking and curing. The paper is then rewetted to return the moisture content to 7.3%, and then compounded with a release layer material to obtain a graphically coated high-performance paper substrate silicone protective film.
[0088] The obtained protective film has a dry adhesive thickness of 9 μm, a pattern edge straightness tolerance of 0.44 mm, and an adhesive surface glossiness Gu value (60°) of 73.2.
[0089] Example 9
[0090] 80 parts of silicone oil (viscosity of 1800cps, vinyl content of 0.35%), 20 parts of high-viscosity silicone glue (solid content of 75%, viscosity of 3500cps), 12 parts of toluene as a diluent, 1.5 parts of a cross-linking agent (syl-offSL7028; Dow Corning), 0.1 parts of an inhibitor (methyl butynol, 98%; Aladdin reagent), and 1.5 parts of a catalyst (syl-off4000; Dow Corning) were added under stirring and mixed to obtain a pressure-sensitive adhesive with a solid content of 85.2% and a glue viscosity of 1800cps. The obtained glue is graphically coated on coated paper with a moisture content of 7.5% using an 80-mesh gravure screen roll through a gravure printing process, leveled for 180 seconds at room temperature, and then placed in an oven for drying and curing. The highest point of the oven temperature is set at 130°C to ensure effective cross-linking and curing. The paper is then rewetted to return the moisture content to 7.3%, and then compounded with a release layer material to obtain a graphically coated high-performance paper substrate silicone protective film.
[0091] The obtained protective film has a dry adhesive thickness of 10 μm, a pattern edge straightness tolerance of 0.41 mm, and an adhesive surface glossiness Gu value (60°) of 68.1.
[0092] Comparative Example 1
[0093] The glue ratio is the same as that in Example 1, but no diluent is added in the ratio, and the obtained pressure-sensitive adhesive has a solid content of 91% and a viscosity of 4500 cps. The patterned coating process is the same as that in Example 1.
[0094] The obtained protective film has a dry adhesive thickness of 16 μm, a pattern edge straightness tolerance of 0.32 mm, and an adhesive surface glossiness Gu value (60°) of 59.8.
[0095] Comparative Example 2
[0096] The glue ratio is the same as that in Example 1, and the patterned coating process is the same as that in Example 1, but the room temperature leveling support is shortened from 300s to 10s.
[0097] The obtained protective film has a dry adhesive thickness of 15 μm, a pattern edge straightness tolerance of 0.34 mm, and an adhesive surface glossiness Gu value (60°) of 63.1.
[0098] Comparative Example 3
[0099] The glue ratio is the same as that in Example 5, and the amount of the diluent added is changed to 25 parts. The obtained pressure-sensitive adhesive has a solid content of 77.5% and a viscosity of 550 cps. The patterned coating process is the same as that in Example 5.
[0100] The obtained protective film has a dry adhesive thickness of 4 μm, a pattern edge straightness tolerance of 0.78 mm, and an adhesive surface glossiness Gu value (60°) of 49.1.
[0101] Comparative Example 4
[0102] The glue ratio is the same as that in Example 5, and the patterned coating process is the same as that in Example 5, but the room temperature leveling support is extended from 180s to 450s.
[0103] The obtained protective film has a dry adhesive thickness of 5 μm, a pattern edge straightness tolerance of 1.12 mm, and an adhesive surface glossiness Gu value (60°) of 62.6.
[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-precision graphic coated silicone protective film, which consists of a silicone pressure-sensitive adhesive layer and a printing substrate. The organic silicon pressure-sensitive adhesive layer is graphically printed on a printing substrate, the printing substrate is divided into a corresponding screen portion and a handle portion connected to each other, the organic silicon pressure-sensitive adhesive layer covers the corresponding screen portion of the printing substrate, and the handle portion of the printing substrate is a non-adhesive area; The straightness tolerance of the edge area of the organic silicone pressure-sensitive adhesive layer is less than 1 mm, the surface of the organic silicone pressure-sensitive adhesive layer is smooth and flat, and the glossiness Gu value of the adhesive surface is 65-100, and the Gu value is measured at 60°; The total mass proportion of the diluent in the pressure-sensitive adhesive of the silicone pressure-sensitive adhesive layer does not exceed 35%, and the viscosity of the pressure-sensitive adhesive is between 500-5000cps; the composition ratio of the pressure-sensitive adhesive is as follows in parts by weight: 50-90 parts of silicone oil; 10-50 parts of high-viscosity silicone glue; 1-3 parts of cross-linking agent; 0.05-0.2 parts of inhibitor; 0-15 parts of diluent, and the amount of diluent is not 0; 0.5-2 parts of catalyst; The viscosity of the silicone oil is 500 cps to 10,000 cps, and the vinyl mole fraction is 0.10% to 0.60%; The high-viscosity silicone glue is a silicone rubber solution modified by MQ resin, with a solid content of 65-80%, and the remaining components are diluents; The pressure-sensitive adhesive is graphically transferred to the printing substrate through a screen with a customized pattern by a silk screen or a gravure printing process; the pressure-sensitive adhesive transferred to the printing substrate is subjected to a 20-300s room temperature leveling process to fully fuse and level the pixel matrix of the pressure-sensitive adhesive.
2. The high-precision patterned coated silicone protective film according to claim 1, wherein: The thickness of the organic silicon pressure-sensitive adhesive layer is 5-20 μm.
3. The high-precision patterned coated silicone protective film according to claim 1, wherein: The printing substrate is a smooth, flat, liquid-impermeable polymer film.
4. The high-precision patterned coated silicone protective film according to claim 1, wherein: The printing substrate is a paper substrate.
5. The high-precision patterned coated silicone protective film according to claim 4, wherein: The total mass of the diluent in the pressure-sensitive adhesive of the organic silicone pressure-sensitive adhesive layer accounts for 5-18%, and the viscosity of the pressure-sensitive adhesive is between 800-3000 cps.
6. The high-precision patterned coated silicone protective film according to claim 4, wherein: The pressure-sensitive adhesive composition ratio of the organic silicone pressure-sensitive adhesive layer is as follows by weight: 70-90 parts of silicone oil; 10-30 parts of high-viscosity silicone glue; 0-15 parts of diluent, and the amount of diluent is not 0; 1-3 parts of cross-linking agent; 0.05-0.2 parts of inhibitor; and 0.5-2 parts of catalyst.
7. A method for preparing a high-precision patterned coated silicone protective film according to any one of claims 1 to 3, comprising the following steps: (1) weighing silicone oil, high-viscosity silicone glue, diluent, cross-linking agent, inhibitor, and catalyst according to the formula amount, and mixing them evenly to obtain a pressure-sensitive adhesive glue; (2) Graphically transferring the pressure-sensitive adhesive to the substrate through a screen with a custom pattern by silk-screen or gravure printing; (3) The pressure-sensitive adhesive transferred to the printing substrate undergoes a 20-300s room temperature leveling process to allow the pixel matrix of the pressure-sensitive adhesive to be fully integrated and leveled; (4) The pressure-sensitive adhesive that has undergone the leveling process enters an oven, where the solvent is volatilized and a curing reaction occurs simultaneously at a high temperature of 90 to 160° C., forming a silicone pressure-sensitive adhesive layer; (5) A release layer is bonded to the adhesive surface of the silicone pressure-sensitive adhesive layer to obtain a high-precision patterned coated silicone protective film.
8. A method for preparing a high-precision patterned coated silicone protective film as claimed in any one of claims 4 to 6, comprising the following steps: (1) weighing silicone oil, high-viscosity silicone glue, diluent, cross-linking agent, inhibitor, and catalyst according to the formula amount, and mixing them evenly to obtain a pressure-sensitive adhesive glue; (2) Graphically transferring the pressure-sensitive adhesive to the printing paper substrate through a screen with a customized pattern by silk-screen or gravure printing; (3) The pressure-sensitive adhesive transferred to the printing paper substrate undergoes a low-temperature leveling process of 30 to 300 seconds, so that the pixel matrix of the pressure-sensitive adhesive is fully integrated and leveled; (4) The patterned pressure-sensitive adhesive that has undergone the leveling process enters an oven, where the solvent evaporates and a curing reaction occurs simultaneously at a high temperature of 90 to 160° C., forming a silicone pressure-sensitive adhesive layer; (5) rewetting the printing paper substrate; (6) A release layer is bonded to the adhesive surface of the silicone pressure-sensitive adhesive layer to obtain a high-precision patterned coated silicone protective film.