Multifunctional solid acid catalyst coupled with polyacid and its preparation method and application

CN115920877BActive Publication Date: 2024-11-08NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211547258.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-11-08
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

[0005]为此,本发明所要解决的技术问题在于提供多酸耦合多功能固体酸催化剂及其制备方法和应用,以解决现有固体酸催化剂在催化生物质原料转化为乳酸时,乳酸产率低、循环稳定性差等问题

Benefits of technology

[0021] The preparation method of the present invention can be used to prepare a multi-acid coupling multifunctional solid acid catalyst with a higher yield, and the solid acid catalyst can efficiently and stably hydrolyze different biomass raw materials into lactic acid, and at the same time, the catalyst can be easily separated from the reaction liquid It is separated from the catalyst and is an environmentally friendly catalyst that can be recycled. Catalyzing the hydrolysis of biomass raw materials under mild reaction conditions, the lactic acid yield can reach 67.8% when using crop waste corncob powder as raw material. In addition, the catalyst also shows excellent catalytic effect in original biomass raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920877B_ABST
    Figure CN115920877B_ABST
Patent Text Reader

Abstract

The invention discloses a multi-acid coupled multifunctional solid acid catalyst and a preparation method and application thereof. The chemical structural formula of the catalyst is Ln a Nb b O x , Ln is one or two of the lanthanide metal elements; the ratio of the amount of substance a of the lanthanide metal element Ln to the amount of substance b of the niobium element is 1 to 3:1, and x is 4 to 7. The preparation method thereof is as follows: adding hydrated niobium pentoxide to a hydrogen peroxide solution, mixing well, placing in an ice water bath, and adding ammonia water; reacting to obtain (NH4)3[Nb(O2)4]; adding (NH4)3[Nb(O2)4] to a lanthanide metal nitrate aqueous solution, aging at room temperature after sufficient reaction, filtering, separating and drying to obtain a solid product; and calcining the solid product. The solid acid catalyst is used to hydrolyze biomass raw materials to produce lactic acid. The present invention can solve the problems of low lactic acid yield and poor cycle stability of existing catalysts when catalyzing the production of lactic acid from biomass raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid acid catalysts, in particular to a multi-acid coupled multifunctional solid acid catalyst and a preparation method and application thereof. Background Art

[0002] In today's world, the rapid growth of the world's population has dramatically increased the demand for energy and chemicals. Traditional non-renewable resources, especially fossil resources, coal and oil, will gradually decrease and have a serious impact on the environment and climate. Therefore, finding sustainable resources to replace fossil resources is the main research direction. Biomass resources, as an emerging alternative to fossil energy, have attracted widespread attention.

[0003] As an important biomass-based platform chemical, lactic acid is widely used in many fields such as food, medicine, chemical industry and pesticide. With the rapid increase in market demand for lactic acid, it is of great scientific significance to find environmentally friendly chemical catalytic methods to convert biomass into lactic acid. At present, many solid catalyst systems have been developed to convert biomass raw materials into small molecule chemical lactic acid.

[0004] The traditional fermentation method for producing lactic acid has problems with waste disposal, high separation costs, and the inability to convert cellulose and hemicellulose without expensive pretreatment. The main way is to adjust the pH value of sugar to about 5 under the action of lactic acid bacteria, and ferment for three to five days to obtain crude lactic acid. The raw materials of the fermentation method are generally starchy raw materials such as corn, rice, and sweet potatoes (some also use alfalfa, cellulose, etc. as raw materials, and some studies have proposed the recycling of kitchen waste and fish waste to produce lactic acid). In contrast, chemical catalysis is considered to be an effective method for upgrading biomass hemicellulose to selective value-added chemicals. Although the catalyst can catalyze the production of lactic acid from biomass under hydrothermal conditions, obtaining a high yield of lactic acid is still the main challenge. Therefore, it is necessary to develop a solid catalyst that can be recycled and efficiently convert biomass raw materials into lactic acid. Summary of the invention

[0005] To this end, the technical problem to be solved by the present invention is to provide a multi-acid coupled multifunctional solid acid catalyst and its preparation method and application, so as to solve the problems of low lactic acid yield and poor cyclic stability of existing solid acid catalysts when catalyzing the conversion of biomass raw materials into lactic acid.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] Multifunctional solid acid catalyst coupled with polyacid, the chemical structure is Ln a Nb b O x, Ln is one or two of the lanthanide metal elements; the ratio of the amount a of the lanthanide metal element Ln to the amount b of the niobium element is 1 to 3:1, and x is 4 to 7. The multi-acid coupled multifunctional solid acid catalyst of the present invention couples the Lewis acid and the Bronsted acid site and different acid sites, and controls the ratio of the amount b of the lanthanide metal element Ln a to the amount b of the niobium element to be 1 to 3:1, so that the acid content and the acid strength of the Lewis acid and the Bronsted acid are optimized.

[0008] The preparation method of a multi-acid coupled multifunctional solid acid catalyst comprises the following steps:

[0009] Step (1), adding hydrated niobium pentoxide Nb2O5·nH2O to a hydrogen peroxide solution and mixing to obtain a mixed system A; placing the mixed system A in an ice water bath, and adding ammonia water to the mixed system A for reaction, after the reaction is completed, washing and drying the obtained reaction product in sequence to obtain (NH4)3[Nb(O2)4];

[0010] Step (2), adding (NH4)3[Nb(O2)4] to an aqueous solution of lanthanide metal nitrate, vigorously stirring and mixing to fully react, and obtaining a mixed system B after the reaction is completed; aging the mixed system B at room temperature, and then filtering and separating in sequence; drying the separated precipitate to obtain a solid product; the purpose of aging is, on the one hand, to allow the components in the mixed system B to fully react, and on the other hand, to completely settle the suspended matter in the mixed system B;

[0011] Step (3), calcining the solid product, and cooling the solid product in the furnace after calcination to obtain a polyacid coupled multifunctional solid acid catalyst; the chemical structural formula of the polyacid coupled multifunctional solid acid catalyst is Ln a Nb b O x , Ln is one or two of the lanthanide metal elements; the ratio of the amount a of the lanthanide metal element Ln to the amount b of the niobium element is 1 to 3:1, and x is 4 to 7.

[0012] In the preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (1), the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 20-30wt%; the concentration of hydrated niobium pentoxide Nb2O5·nH2O in the mixed system A is 0.15-0.65mol / L, and the value of n is 2-5; the mass fraction of NH3 in the ammonia water is 20-30wt%; the volume ratio of ammonia water to hydrogen peroxide solution is 1:(2-8); and the reaction time is 5-10min. If the concentration of ammonia water is too low, it cannot fully react to form a precipitate.

[0013] The preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (1), the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30wt%; the concentration of hydrated niobium pentoxide Nb2O5·nH2O in the mixed system A is 0.156mol / L, and the value of n is 3; the mass fraction of NH3 in the ammonia water is 28wt%; the volume ratio of ammonia water to hydrogen peroxide solution is 1:8; and the reaction time is 10min.

[0014] The preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (2), the molar concentration of lanthanide metal ions in the lanthanide metal nitrate aqueous solution is 0.3-0.65 mol / L; the lanthanide metal nitrate is one or two of La(NO3)3, Ce(NO3)3, Pr(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Ho(NO3)3, Er(NO3)3, Tm(NO3)3 or Yb(NO3)3; the molar ratio of lanthanide metal nitrate to hydrated niobium pentoxide Nb2O5·nH2O is 2:1.

[0015] In the preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (2), the aging time is 2 to 5 hours, the drying temperature of the precipitate is 70 to 85° C., and the drying time is 8 to 12 hours.

[0016] In the preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (2), the aging time is 3 hours, the drying temperature of the precipitate is 80° C., and the drying time is 10 hours.

[0017] In the preparation method of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, in step (3), the solid product is placed in a muffle furnace, and the temperature is increased to 200-1200°C at a heating rate of 5°C / min for constant temperature calcination, and the calcination time is 3-6h.

[0018] The application of the polyacid coupled multifunctional solid acid catalyst is to hydrolyze the biomass raw material into lactic acid using the polyacid coupled multifunctional solid acid catalyst.

[0019] In the application of the above-mentioned multi-acid coupled multifunctional solid acid catalyst, the biomass raw material is one of corn cobs, peanut stalks, wheat straws, cotton stalks, peanut shells, sawdust, cellulose or sycamore wood.

[0020] The technical solution of the present invention achieves the following beneficial technical effects:

[0021] The preparation method of the present invention can prepare a multi-acid coupled multifunctional solid acid catalyst with a high yield, and the solid acid catalyst can efficiently and stably hydrolyze different biomass raw materials into lactic acid. At the same time, the catalyst is easy to separate from the reaction solution and is a recyclable environmentally friendly catalyst. Under mild reaction conditions, the biomass raw material is catalyzed to hydrolyze, and the yield of lactic acid can reach 67.8% when corn cob powder, a crop waste, is used as the raw material. In addition, the catalyst also exhibits excellent catalytic effect in the original biomass raw material.

[0022] The present invention constructs a highly efficient solid acid catalyst containing lanthanide metal ions and having a unique structure, excellent performance and good hydrothermal stability. The solid acid catalyst is a multi-acid coupled multifunctional solid acid catalyst that can selectively convert some actual biomass raw materials into lactic acid. The multi-acid coupled multifunctional solid acid catalyst of the present invention can efficiently convert agricultural waste corn cob powder into lactic acid under hydrothermal conditions, and the substrate can be extended to a variety of other biomass raw materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The XRD pattern of the multi-acid coupled multifunctional solid acid catalyst prepared in the embodiment of the present invention (in the figure, a is YbNbO x , b is YbNbO x -200, c is YbNbO x -400, d is YbNbO x -800, e is YbNbO x -1000, f is YbNbO x -1200);

[0024] Figure 2 Fourier transform infrared spectrum FTIR of the multi-acid coupled multifunctional solid acid catalyst prepared in the embodiment of the present invention (in the figure, a is YbNbO x , b is YbNbO x -200, c is YbNbO x -400, d is YbNbO x -800, e is YbNbO x -1000, f is YbNbO x -1200);

[0025] Figure 3 SEM image of the multi-acid coupled multifunctional solid acid catalyst prepared in the embodiment of the present invention (in the figure, a is YbNbO x , b is YbNbO x -200, c is YbNbO x -400, d is YbNbO x -800, e is YbNbOx -1000, f is YbNbO x -1200);

[0026] Figure 4 The XRD patterns of the multi-acid coupled multifunctional solid acid catalyst prepared in the embodiment of the present invention before and after use. DETAILED DESCRIPTION

[0027] Example 1

[0028] The preparation method of the polyacid coupled multifunctional solid acid catalyst of this embodiment comprises the following steps:

[0029] Step (1), adding 2.0 g (6.25 mmol) of hydrated niobium pentoxide Nb2O5·nH2O to 40.0 mL of hydrogen peroxide solution and mixing to obtain a mixed system A, wherein the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30 wt %; placing the mixed system A in an ice water bath, and adding 5.0 mL of ammonia water to the mixed system A to react for 10 min, wherein the mass fraction of NH3 in the ammonia water is 28 wt %; after the reaction is completed, washing and drying the obtained reaction product in sequence [washing with deionized water and drying at room temperature for 10 h] to obtain (NH4)3[Nb(O2)4];

[0030] Step (2), add (NH4)3[Nb(O2)4] to 20mL Yb(NO3)3 aqueous solution, the amount of Yb(NO3)3·5H2O in the Yb(NO3)3 aqueous solution is 12.5mmol; stir vigorously to mix to make it fully react, during the reaction, [Nb(O2)4] 3- Yb 3+ The reaction was carried out to form a light yellow precipitate insoluble in water, and a mixed system B was obtained after the reaction was completed; the mixed system B was aged at room temperature for 3 hours, and then filtered and separated, and the separated precipitate was dried at 80°C for 10 hours to obtain a solid product, namely YbNbO x Precursor;

[0031] Step (3), solid product YbNbO x The precursor was placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min for constant temperature calcination for 3 hours. After calcination, the furnace was cooled to obtain a multifunctional solid acid catalyst having both Lewis acid and Bronsted acid, which was recorded as YbNbO x -1000;

[0032] The chemical structural formula of the multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is Yb3NbO7.

[0033] Example 2

[0034] The preparation method of the polyacid coupled multifunctional solid acid catalyst of this embodiment comprises the following steps:

[0035] Step (1), adding 2.0 g (6.25 mmol) of hydrated niobium pentoxide Nb2O5·nH2O to 40.0 mL of hydrogen peroxide solution and mixing to obtain a mixed system A, wherein the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30 wt %; placing the mixed system A in an ice water bath, and adding 5.0 mL of ammonia water to the mixed system A to react for 10 min, wherein the mass fraction of NH3 in the ammonia water is 28 wt %; after the reaction is completed, washing and drying the obtained reaction product in sequence [washing with deionized water and drying at room temperature for 10 h] to obtain (NH4)3[Nb(O2)4];

[0036] Step (2), add (NH4)3[Nb(O2)4] to 20mL Sm(NO3)3 aqueous solution, the amount of Sm(NO3)3·5H2O in the Sm(NO3)3 aqueous solution is 12.5mmol; stir vigorously to mix and make it fully react. During the reaction, [Nb(O2)4] 3- Easy to react with trivalent Sm 3+ The reaction was carried out to form a light yellow precipitate insoluble in water, and a mixed system B was obtained after the reaction was completed; the mixed system B was aged at room temperature for 3 hours, and then filtered and separated, and the separated precipitate was dried at 80°C for 10 hours to obtain a solid product, namely SmNbO x Precursor;

[0037] Step (3), solid product SmNbO x The precursor was placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min for constant temperature calcination for 3 hours. After calcination, the furnace was cooled to obtain a multi-acid coupled multifunctional solid acid catalyst having both Lewis acid and Bronsted acid, which was recorded as SmNbO x -1000;

[0038] The chemical structural formula of the polyacid coupled multifunctional solid acid catalyst prepared in this embodiment is Sm3NbO7.

[0039] Example 3

[0040] The preparation method of the polyacid coupled multifunctional solid acid catalyst of this embodiment comprises the following steps:

[0041] Step (1), adding 2.0 g (6.25 mmol) of hydrated niobium pentoxide Nb2O5·nH2O to 40.0 mL of hydrogen peroxide solution and mixing to obtain a mixed system A, wherein the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30 wt %; placing the mixed system A in an ice water bath, and adding 5.0 mL of ammonia water to the mixed system A to react for 10 min, wherein the mass fraction of NH3 in the ammonia water is 28 wt %; after the reaction is completed, washing and drying the obtained reaction product in sequence [washing with deionized water and drying at room temperature for 10 h] to obtain (NH4)3[Nb(O2)4];

[0042] Step (2), add (NH4)3[Nb(O2)4] to 20mL Ho(NO3)3 aqueous solution, the amount of Ho(NO3)3·5H2O in the Ho(NO3)3 aqueous solution is 12.5mmol; stir vigorously to mix to make it fully react. During the reaction, [Nb(O2)4] 3- Easy with trivalent Ho 3+ The reaction was carried out to form a light yellow precipitate insoluble in water, and a mixed system B was obtained after the reaction was completed; the mixed system B was aged at room temperature for 3 hours, filtered and separated, and the separated precipitate was dried at 80°C for 10 hours to obtain a solid product, namely HoNbO x Precursor;

[0043] Step (3), solid product HoNbO x The precursor was placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min for constant temperature calcination for 3 hours. After calcination, the furnace was cooled to obtain a multi-acid coupled multifunctional solid acid catalyst having both Lewis acid and Bronsted acid, which was recorded as HoNbO x -1000;

[0044] The chemical structural formula of the multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is Ho3NbO7.

[0045] Example 4

[0046] The preparation method of the polyacid coupled multifunctional solid acid catalyst of this embodiment comprises the following steps:

[0047] Step (1), adding 2.0 g (6.25 mmol) of hydrated niobium pentoxide Nb2O5·nH2O to 40.0 mL of hydrogen peroxide solution and mixing to obtain a mixed system A, wherein the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30 wt %; placing the mixed system A in an ice water bath, and adding 5.0 mL of ammonia water to the mixed system A to react for 10 min, wherein the mass fraction of NH3 in the ammonia water is 28 wt %; after the reaction is completed, washing and drying the obtained reaction product in sequence with [washing with deionized water and drying at room temperature for 10 h] to obtain (NH4)3[Nb(O2)4];

[0048] Step (2), add (NH4)3[Nb(O2)4] to 20mL La(NO3)3 aqueous solution, the amount of La(NO3)3·5H2O in the La(NO3)3 aqueous solution is 12.5mmol; stir vigorously to mix to make it fully react, during the reaction, [Nb(O2)4] 3- Easy to use with trivalent La 3+ The reaction was carried out to form a light yellow precipitate insoluble in water, and a mixed system B was obtained after the reaction was completed; the mixed system B was aged at room temperature for 3 hours, filtered and separated, and the separated precipitate was dried at 80°C for 9 hours to obtain a solid product, namely LaNbO x Precursor;

[0049] Step (3), solid product LaNbO x The precursor was placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min for constant temperature calcination for 3 hours. After calcination, the furnace was cooled to obtain a multi-acid coupled multifunctional solid acid catalyst having both Lewis acid and Bronsted acid, which was recorded as LaNbO x -1000;

[0050] The chemical structural formula of the polyacid coupled multifunctional solid acid catalyst prepared in this embodiment is La3NbO7.

[0051] Example 5

[0052] The preparation method of the solid acid catalyst in this embodiment is different from that in embodiment 1 only in that the solid product prepared in step (2) is not calcined and is directly used as a solid acid catalyst, denoted as YbNbO x .

[0053] Example 6

[0054] The preparation method of the solid acid catalyst in this embodiment is different from that in embodiment 1 only in that in step (3), the calcination temperature is 200° C. The multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is denoted as YbNbO x -200.

[0055] Example 7

[0056] The preparation method of the solid acid catalyst in this embodiment is different from that in embodiment 1 only in that in step (3), the calcination temperature is 400° C. The multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is denoted as YbNbO x -400.

[0057] Example 8

[0058] The preparation method of the solid acid catalyst in this embodiment is different from that in embodiment 1 only in that in step (3), the calcination temperature is 800° C. The multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is denoted as YbNbO x -800.

[0059] Example 9

[0060] The preparation method of the solid acid catalyst in this embodiment is different from that in embodiment 1 only in that in step (3), the calcination temperature is 1200° C. The multi-acid coupled multifunctional solid acid catalyst prepared in this embodiment is denoted as YbNbO x -1200.

[0061] Example 10

[0062] The preparation method of the solid acid catalyst in this embodiment differs from that in Example 1 only in that:

[0063] In step (2), (NH4)3[Nb(O2)4] is added to 20 mL of Yb(NO3)3 aqueous solution, and the amount of Yb(NO3)3·5H2O in the Yb(NO3)3 aqueous solution is 6.25 mmol. The multi-acid coupled multifunctional solid acid catalyst prepared in this example is denoted as YbNb2O x -1000.

[0064] The structures and morphologies of the solid acid catalysts prepared in Example 1, Example 5, Example 6, Example 7, Example 8 and Example 9 were measured respectively. The results are as follows: Figures 1 to 3 As shown. Figure 1 It can be seen that when the calcination temperature is low, no obvious characteristic diffraction peak of Yb3NbO7 is found, and only the diffraction peak of Nb2O5 (PDF#30-0872) can be observed. When the calcination temperature is increased to 800°C, the diffraction peak of Yb3NbO7 appears, and its specific diffraction peaks are located at 29.7, 34.5, 49.6, and 58.9°. Further increasing the calcination temperature, another crystalline phase is gradually formed, and the crystal form of the composite oxide gradually changes from Yb3NbO7 to YbNbO4. When the calcination temperature of the catalyst is increased to 1200°C, YbNbO4 is the main component. Figure 2It can be seen that with the increase of calcination temperature, the structure of the catalyst changes to a certain extent, mainly because its crystal form changes to a certain extent. Figure 3 It can be seen that with the increase of calcination temperature, the surface morphology of the catalyst changes. When the calcination temperature increases to 1200℃, the surface of the catalyst becomes smooth.

[0065] The solid acid catalysts prepared in Example 1, Example 2, Example 3 and Example 4 were used to catalyze the hydrolysis of agricultural waste corncob powder into lactic acid. The specific catalytic methods are as follows:

[0066] Take 0.1g corncob powder and 0.03g prepared catalyst Ln a Nb b O x -1000, add 12.00mL of deionized water, and put it into a high-pressure reactor. Replace the gas in the reactor with high-purity nitrogen three times, and then fill it with 2.0MPa nitrogen as a protective gas, and react for 30 minutes at 240°C. Take the reaction solution and use a high-performance liquid chromatograph for qualitative and quantitative analysis. The results are shown in Table 1.

[0067] Table 1Ln a Nb b O x Calculation results of the yield of lactic acid produced from corncob powder catalyzed by -1000 catalyst

[0068]

[0069]

[0070] The solid acid catalysts prepared in Examples 5, 6, 7, 8 and 9 were used to catalyze the hydrolysis of agricultural waste corncob powder into lactic acid. The specific catalytic methods are as follows:

[0071] Take 0.1g corncob powder and 0.03g of the prepared catalyst, add 12.00mL of deionized water, and put it into a high-pressure reactor. Replace the gas in the reactor with high-purity nitrogen three times, then fill it with 2.0MPa nitrogen as a protective gas, and react at 240℃ for 30min. Take the reaction liquid and use a high-performance liquid chromatograph for qualitative and quantitative analysis. The results are shown in Table 2.

[0072] Table 2 Calculation results of the yield of lactic acid produced by corncob powder catalyzed by catalyst

[0073] Solid acid catalyst Lactic acid yield (%) <![CDATA[Example 5: YbNbO x > 46.6 <![CDATA[Example 6: YbNbO x -200]]> 50.4 <![CDATA[Example 7: YbNbO x -400]]> 51.6 <![CDATA[Example 8: YbNbO x -800]]> 56.0 <![CDATA[Example 9: YbNbO x -1200]]> 21.5

[0074] The solid acid catalyst prepared in Example 1 is used to catalyze the hydrolysis of corn cob powder into lactic acid, and the specific method is as follows:

[0075] The yield of the product was improved by changing the mass ratio of the substrate corncob powder and the catalyst. 0.1 g of corncob powder and a certain amount of the catalyst YbNbO prepared in Example 1 were added. x -1000, add 12.00mL of deionized water, and put it into a high-pressure reactor. Replace the gas in the reactor with high-purity nitrogen three times, and then fill it with 2.0MPa nitrogen as a protective gas, and react for 30 minutes at 240°C. Take the reaction solution and use a high-performance liquid chromatograph for qualitative and quantitative analysis. The results are shown in Table 3.

[0076] Table 3 Calculation results of the yield of lactic acid produced by different ratios of corncob powder and catalyst

[0077]

[0078]

[0079] In order to compare the catalytic effects of Example 1 and Example 10 in catalyzing the hydrolysis of corn cob powder into lactic acid, the researchers of the present invention also conducted the following experiments:

[0080] The yield of the product was improved by changing the ratio of ytterbium and niobium in the catalyst. 0.1 g of corn cob powder and a certain amount of the prepared catalyst were taken, 12.00 mL of deionized water was added, and the mixture was placed in a high-pressure reactor. The gas in the reactor was replaced three times with high-purity nitrogen, and then 2.0 MPa of nitrogen was filled as a protective gas, and the reaction was carried out at 240 ° C for 30 minutes. The reaction solution was tested with a high-performance liquid chromatograph for qualitative and quantitative analysis. The results are shown in Table 4.

[0081] Table 4 Calculation results of the yield of lactic acid produced from corncob powder catalyzed by catalysts with different ytterbium contents

[0082] Solid acid catalyst Lactic acid yield (%) <![CDATA[Example 1: YbNbO x -1000]]> 67.8 <![CDATA[Example 10: YbNb2O x -1000]]> 38.5

[0083] The solid acid catalyst prepared in Example 1 was used to catalyze the hydrolysis of different biomass raw materials [peanut stalks, wheat stalks, cotton stalks, peanut shells, sawdust, sycamore wood and cellulose] into lactic acid. The specific catalytic method is as follows:

[0084] Take 0.1g of one of the biomass raw materials and 0.03g of catalyst YbNbOx-1000, add 12.00mL of deionized water, and put it into a high-pressure reactor. Replace the gas in the reactor with high-purity nitrogen three times, then fill it with 2.0MPa nitrogen as a protective gas, and react at 240℃ for 30min. Take the reaction liquid for detection by high-performance liquid chromatography, and perform qualitative and quantitative analysis. The results are shown in Table 5.

[0085] Table 5 Liquid phase analysis results of lactic acid production from raw biomass catalyzed by YbNbOx catalyst

[0086]

[0087]

[0088] The solid acid catalyst prepared in Example 1 was used for the catalyst cycle stability test, and the specific method was as follows:

[0089] Take 0.1 g corn cob powder and the catalyst YbNbO prepared in Example 1 x -1000 0.03g, add 12.00mL of deionized water, and put it into a high-pressure reactor. Replace the gas in the reactor with high-purity nitrogen three times, then fill it with 2.0MPa nitrogen as a protective gas, and react for 30min at 240℃. Take the reaction liquid and test it with a high-performance liquid chromatograph for qualitative and quantitative analysis. After centrifugation, filtration, washing and drying, the solid catalyst is added to the reactor again to catalyze the hydrolysis of corn cob powder again. The results are shown in Table 6. Figure 4 XRD spectra of the fresh catalyst and the catalyst after reaction cycle.

[0090] Table 6 Cyclic performance of YbNbOx-1000 catalyst

[0091] Cycle times Lactic acid yield (%) 1 67.8 2 62.6 3 58.9

[0092] Figure 4 It can be found that the characteristic diffraction peaks of the XRD spectrum of the catalyst after the reaction (used) have not changed significantly compared with those of the fresh catalyst (fresh), indicating that the catalyst has good stability.

[0093] In summary, the multi-active component solid acid catalyst modified with lanthanide metals proposed in the present invention can be used for the efficient conversion of biomass raw materials into lactic acid; by measuring the structure and morphology of the catalyst, investigating the effects of different lanthanide metal ions, different calcination temperatures, different metal ratios, etc. on the catalytic reaction activity, and using a high-temperature and high-pressure reactor to evaluate the activity of the prepared catalyst, the results show that the catalyst prepared by the present invention can effectively convert biomass raw materials into lactic acid, and when certain biomass raw materials are used as substrates, it exhibits high catalytic activity and has good selectivity. In addition, the preparation method of the present invention is used to prepare a multi-acid coupled multifunctional solid acid catalyst with a high yield, which can effectively control the production cost of the multi-acid coupled multifunctional solid acid catalyst.

[0094] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.

Claims

1. Application of multi-acid coupled multifunctional solid acid catalyst, characterized in that: The biomass raw material is hydrolyzed into lactic acid by a multi-acid coupled multifunctional solid acid catalyst, wherein the biomass raw material is one of corn cobs, peanut stalks, wheat straws, cotton stalks, peanut shells, sawdust, cellulose or sycamore wood; The chemical formula of the multifunctional solid acid catalyst coupled with polyacid is Ln a Nb b O x , Ln is one or two of the lanthanide metal elements; the ratio of the amount a of the lanthanide metal element Ln to the amount b of the niobium element is 1 to 3:1, and x is 4 to 7; The preparation method of a multi-acid coupled multifunctional solid acid catalyst comprises the following steps: Step (1), adding hydrated niobium pentoxide Nb2O5·nH2O to a hydrogen peroxide solution and mixing well to obtain a mixed system A; placing the mixed system A in an ice water bath, and adding ammonia water to the mixed system A for reaction, after the reaction is completed, washing and drying the obtained reaction product in sequence to obtain (NH4)3[Nb(O2)4]; Step (2), adding (NH4)3[Nb(O2)4] to the aqueous solution of lanthanide metal nitrate, vigorously stirring and mixing to fully react, and obtaining a mixed system B after the reaction is completed; aging the mixed system B at room temperature, and then filtering and separating in sequence; drying the separated precipitate to obtain a solid product; Step (3), calcining the solid product, and cooling it in the furnace after calcination to obtain a polyacid coupled multifunctional solid acid catalyst.

2. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 1, characterized in that: In step (1), the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 20-30wt%; the concentration of hydrated niobium pentoxide Nb2O5·nH2O in the mixed system A is 0.15-0.65 mol / L, and the value of n is 2-5; the mass fraction of NH3 in the ammonia water is 20-30wt%; the volume ratio of ammonia water to hydrogen peroxide solution is 1:(2-8); and the reaction time is 5-10 min.

3. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 2, characterized in that: In step (1), the mass fraction of hydrogen peroxide in the hydrogen peroxide solution is 30wt%; the concentration of hydrated niobium pentoxide Nb2O5·nH2O in the mixed system A is 0.156mol / L; the mass fraction of NH3 in the ammonia water is 28wt%; the volume ratio of ammonia water to hydrogen peroxide solution is 1:8; and the reaction time is 10 min.

4. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 1, characterized in that: In step (2), the molar concentration of lanthanide metal ions in the lanthanide metal nitrate aqueous solution is 0.3-0.65 mol / L; the lanthanide metal nitrate is one or two of La(NO3)3, Ce(NO3)3, Pr(NO3)3, Sm(NO3)3, Eu(NO3)3, Gd(NO3)3, Tb(NO3)3, Dy(NO3)3, Ho(NO3)3, Er(NO3)3, Tm(NO3)3 or Yb(NO3)3; and the molar ratio of the lanthanide metal nitrate to hydrated niobium pentoxide Nb2O5·nH2O is 2:

1.

5. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 1, characterized in that: In step (2), the aging time is 2 to 5 hours, the drying temperature of the precipitate is 70 to 85° C., and the drying time is 8 to 12 hours.

6. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 5, characterized in that: In step (2), the aging time is 3 hours, the drying temperature of the precipitate is 80° C., and the drying time is 10 hours.

7. The use of the multi-acid coupled multifunctional solid acid catalyst according to claim 1, characterized in that: In step (3), the solid product is placed in a muffle furnace, and the temperature is raised to 200-1200° C. at a heating rate of 5° C. / min for constant temperature calcination, and the calcination time is 3-6 hours.