A carbon dioxide hydrogenation catalyst and its preparation method and application
By using a combination of natural clay montmorillonite carrier and metal oxide in the carbon dioxide hydrogenation reaction, a solid alkali catalyst loaded with metal nickel is prepared, which solves the problems of insufficient catalyst activity and difficult alkalinity control in the existing technology, and achieves Efficient conversion of carbon dioxide into methane and suitable for industrial production.
Patent Information
- Application Number
- CN202211475116.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The preparation process of existing supported inorganic solid alkali catalysts is complex, with insufficient activity, single distribution form, and difficult alkalinity control. Especially in the hydrogenation of carbon dioxide to methane reaction, the alkalinity control of the catalyst poses great challenges.
Using natural clay montmorillonite as a carrier, through the hydration reaction with cerium or magnesium metal salt and hydroxide, the melting reaction of frozen ice cubes, combined with the treatment of nickel nitrate and sodium hydroxide, a solid alkali catalyst loaded with metal nickel is prepared. Adjust the basicity of the catalyst to improve its performance in carbon dioxide hydrogenation reactions.
The catalytic effect of efficiently converting carbon dioxide into methane under low temperature conditions is achieved. The carbon dioxide conversion rate of the catalyst reaches 32.7%, and 100% methane selectivity is maintained. The preparation method is simple and low-cost, making it suitable for industrial production.
Smart Images

Figure CN115920914B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical industry, and in particular relates to a natural clay-loaded metal oxide solid base catalyst, a method for preparing the catalyst and application of the catalyst in a carbon dioxide hydrogenation to methane reaction. Background Art
[0002] Solid base catalysts, including alkali metal oxides, transition metal oxides, composite oxides and supported oxides (Fuel. 2007, 86: 328–333. Clean Energy. 2019, 3: 2-23.), have high activity, low corrosion, easy separation and anti-toxicity. These advantages have made them widely used in the chemical industry, such as biomass to diesel (Fuel. 2013, 106: 279-284. Chinese invention patent, publication number CN201810558642.1.), carbon dioxide methanation (Catalysis Science & Technology. 2016, 6: 3976–3983.), etc. At present, the preparation process of supported inorganic solid base catalysts is relatively complicated, and there are disadvantages such as insufficient activity, single distribution form, and difficult regulation. In particular, there are still great challenges in alkalinity regulation.
[0003] The large-scale emission of greenhouse gases such as CO2 has disrupted the balance of the global carbon cycle. Hydrogenation of carbon dioxide to methanogens is an ideal way to reduce carbon emissions and alleviate energy shortages, which has very important research significance. For the carbon dioxide methanation reaction, the introduction of certain alkaline components in the process of constructing the catalyst can promote CO2 adsorption and activation (CatalysisToday.2021,368:2-19), and the efficient activation of CO2 is the key to achieving low-temperature CO2 methanation. The alkalinity of the catalyst plays a key role. The preparation of catalysts with controllable alkalinity helps to achieve efficient low-temperature CO2 methanation. Summary of the invention
[0004] The purpose of the present invention is to provide a solid base catalyst.
[0005] Another object of the present invention is to provide a method with low cost and simple process to prepare the above catalyst.
[0006] Another object of the present invention is to provide the use of the above catalyst in the reaction of hydrogenating carbon dioxide to produce methane.
[0007] The above objectives of the present invention are achieved through the following technical solutions.
[0008] The present invention provides a method for preparing a carbon dioxide hydrogenation catalyst, the steps of which are as follows:
[0009] (1) mixing montmorillonite and water in a mass ratio of 1:50 to 100, and stirring at room temperature for 2 to 4 hours to obtain a fully hydrated montmorillonite aqueous solution;
[0010] (2) freezing a cerium or magnesium metal salt solution having a concentration of 0.001 to 0.008 mol / L and a hydroxide solution having a molar ratio of 2 to 3:1 to magnesium salt or cerium salt and a concentration of 0.002 to 0.024 mol / L into ice cubes;
[0011] (3) adding the metal salt solution and hydroxide solution ice cubes obtained in step (2) to the montmorillonite aqueous solution obtained in step (1) in a manner of melting and releasing at room temperature, stirring and reacting while melting until the ice cubes are completely melted, centrifugally washing three times, and drying at 80-100° C. for 8-16 hours to obtain a solid base catalyst precursor;
[0012] (4) calcining the solid base catalyst precursor obtained in step (3) at 450-550° C. in an air atmosphere for 3-6 hours, and cooling to room temperature to obtain a solid base catalyst;
[0013] (5) mixing the solid base catalyst prepared in step (4) with water at a mass ratio of 1:100, and stirring at room temperature for 4 hours to obtain a fully hydrated solid base catalyst aqueous solution;
[0014] (6) freezing a nickel nitrate solution having a nickel nitrate to solid base catalyst mass ratio of 30:100 and a concentration of 0.008 to 0.040 mol / L, and a sodium hydroxide solution having a sodium hydroxide to nickel nitrate molar ratio of 2:1 and a concentration of 0.016 to 0.080 mol / L into ice cubes;
[0015] (7) adding the nickel nitrate solution and sodium hydroxide solution ice cubes obtained in step (6) to the solid base catalyst aqueous solution obtained in step (5) in a manner of melting and releasing at room temperature, stirring and reacting while melting until the ice cubes are completely melted, centrifuging and washing three times, and drying at 100° C. for 12 hours to obtain a solid base-supported nickel hydroxide methane hydrogenation catalyst precursor;
[0016] (8) The solid base supported nickel hydroxide methane hydrogenation catalyst precursor obtained in step (7) is reduced by hydrogen at 550° C. for 4 hours, cooled to room temperature under a hydrogen atmosphere, and then passivated by a mixed gas of O2 / N2 with a volume ratio of 0.5 to 1.0% at room temperature for 4 hours to obtain a carbon dioxide hydrogenation catalyst that can be directly stored in the air.
[0017] Furthermore, the montmorillonite in step (1) is sodium montmorillonite.
[0018] Furthermore, the cerium salt in step (2) is any one of cerium nitrate, cerium chloride and cerium sulfate; and the magnesium salt is magnesium nitrate.
[0019] Furthermore, the cerium salt in step (2) is cerium nitrate.
[0020] Furthermore, the hydroxide in step (2) is sodium hydroxide or potassium hydroxide.
[0021] Furthermore, the hydroxide in step (2) is sodium hydroxide.
[0022] The carbon dioxide hydrogenation catalyst prepared by the above method has natural clay montmorillonite as a carrier, metal oxide cerium oxide or magnesium oxide as a basic component and loaded with metal nickel, and the mass of the metal oxide is 0.5-4wt% of the total mass of the catalyst.
[0023] The carbon dioxide hydrogenation catalyst prepared by the above method can be used in carbon dioxide hydrogenation reaction.
[0024] Furthermore, the carbon dioxide hydrogenation product is methane.
[0025] The carbon dioxide hydrogenation to methane performance of the solid base-supported nickel catalyst of the present invention. The carbon dioxide hydrogenation reaction is carried out in a micro fixed bed reactor. The specific steps and conditions are as follows: 0.25g of the solid base-supported nickel carbon dioxide hydrogenation catalyst is loaded into the fixed bed reactor, H2 is introduced to activate the catalyst at 300°C for 2 hours, the temperature is lowered to the reaction temperature, H2+CO2 reaction gas (H2:CO2=1:4) is introduced to react at 0.25MPa, and the hydrogenation product is sampled and analyzed online using a GC-1690 gas chromatograph using an internal standard method.
[0026] Compared with the prior art, the present invention has the following technical effects:
[0027] (1) CO2 itself has a certain acidity. When the catalytic conversion reaction is carried out, the introduction of alkaline components into the catalyst is conducive to CO2 adsorption and activation, thereby promoting the CO2 conversion performance of the catalyst. The present invention regulates the alkalinity of the catalyst by introducing different loading amounts of CeO2, thereby improving the performance of carbon dioxide hydrogenation to methane of the loaded metal nickel catalyst. Its adjustable alkalinity also greatly broadens the application field of the solid base catalyst.
[0028] (2) The solid base-supported nickel catalyst of the present invention has excellent performance in hydrogenating carbon dioxide to produce methane. At a reaction temperature of 180° C., the carbon dioxide conversion rate reaches 32.7% and maintains 100% methane selectivity.
[0029] (3) The present invention uses the cheap and readily available natural clay montmorillonite as a carrier to prepare a solid base catalyst with controllable alkalinity.
[0030] (4) The catalyst preparation method of the present invention is simple and low-cost, and is very suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is the CO2-TPD diagram of the solid base catalyst of the present invention.
[0032] Figure 2 The XRD diagram of the solid base supported nickel Ni-CeO2 / MMT-4 carbon dioxide hydrogenation catalyst of the present invention. DETAILED DESCRIPTION
[0033] In order to further illustrate the present invention, the following examples are given, but they do not limit the scope of the invention defined by the claims.
[0034] 1. Preparation of solid base catalyst
[0035] Example 1
[0036] Take 1g of sodium montmorillonite and place it in a 250ml beaker, add 100ml of water and stir at room temperature for 2 hours to obtain a fully hydrated montmorillonite aqueous solution. Take 60ml of 0.001mol / L cerium nitrate solution and 60ml of 0.003mol / L potassium hydroxide solution respectively, and freeze them into ice cubes. Add the obtained cerium nitrate solution and potassium hydroxide solution ice cubes into the above montmorillonite aqueous solution stirred by a magnetic stirrer in a way of melting and releasing at room temperature, and stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 80℃ for 16 hours, calcine at 450℃ in air atmosphere for 6 hours, and cool to room temperature to obtain a solid base catalyst, represented by CeO2 / MMT-1.
[0037] Example 2
[0038] Take 1g of sodium montmorillonite and place it in a 250ml beaker, add 75ml of water and stir at room temperature for 3 hours to obtain a fully hydrated montmorillonite aqueous solution. Take 40ml of 0.003mol / L cerium chloride solution and 40ml of 0.009mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. Add the obtained cerium chloride solution and sodium hydroxide solution ice cubes into the above montmorillonite aqueous solution stirred by a magnetic stirrer in a way of melting and releasing at room temperature, and stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 100℃ for 8 hours, calcine at 500℃ in air atmosphere for 5 hours, and cool to room temperature to obtain a solid base catalyst, represented by CeO2 / MMT-2.
[0039] Example 3
[0040] Take 1g of sodium montmorillonite and place it in a 250ml beaker, add 50ml of water and stir at room temperature for 4 hours, and disperse it with ultrasound assistance for 3 hours to obtain a fully hydrated montmorillonite aqueous solution. Take 30ml of 0.006mol / L cerium sulfate solution and 30ml of 0.018mol / L potassium hydroxide solution respectively, and freeze them into ice cubes. The obtained cerium sulfate solution and potassium hydroxide solution ice cubes are added to the above montmorillonite aqueous solution stirred by a magnetic stirrer in a way of melting and releasing at room temperature, and the reaction is stirred while melting until the ice cubes are completely melted, centrifuged and washed 3 times, dried at 90℃ for 12 hours, calcined at 550℃ in air atmosphere for 3 hours, and cooled to room temperature to obtain a solid base catalyst, represented by CeO2 / MMT-3.
[0041] Example 4
[0042] Take 1g of sodium montmorillonite and place it in a 250ml beaker, add 50ml of water and stir at room temperature for 4 hours to obtain a fully hydrated montmorillonite aqueous solution. Take 30ml of 0.008mol / L cerium nitrate solution and 30ml of 0.024mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. Add the obtained cerium nitrate solution and sodium hydroxide solution ice cubes into the above montmorillonite aqueous solution stirred by a magnetic stirrer in a way of melting and releasing at room temperature, and stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 90℃ for 12 hours, calcine at 520℃ in air atmosphere for 4 hours, and cool to room temperature to obtain a solid base catalyst, represented by CeO2 / MMT-4.
[0043] Example 5
[0044] Take 1g of sodium montmorillonite and place it in a 250ml beaker, add 75ml of water and stir at room temperature for 3 hours to obtain a fully hydrated montmorillonite aqueous solution. Take 40ml of 0.003mol / L magnesium nitrate solution and 40ml of 0.006mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. Add the obtained cerium nitrate solution and sodium hydroxide solution ice cubes to the above montmorillonite aqueous solution stirred by a magnetic stirrer in a way of melting and releasing at room temperature, and stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 90℃ for 12 hours, calcine at 520℃ in air atmosphere for 4 hours, and cool to room temperature to obtain a solid base catalyst, expressed as MgO / MMT.
[0045] The alkalinity test (CO2-TPD) of the solid base catalyst of the present invention was carried out on a CHEMBET-300 chemical adsorption instrument of Quantachrome Corporation of the United States. The CO2-TPD results are as follows: Figure 1 As shown. Figure 1It can be seen that the MgO / MMT-catalyst has two obvious CO2 desorption peaks at 380℃ and 500℃, and the peak intensity is significantly greater than that of the CeO2 / MMT-2 catalyst with the same molar amount, indicating that the basicity of the catalyst components is quite different; CeO2 / MMT-1 and CeO2 / MMT-2 catalysts have obvious CO2 desorption peaks near 200℃, indicating that they have weak basicity; CeO2 / MMT-3 and CeO2 / MMT-4 catalysts have obvious CO2 desorption peaks near 380℃, indicating that they have medium-strong basicity; at the same time, with the increase of cerium oxide loading, the corresponding CO2 desorption peak area also increases accordingly, indicating that the number of basic centers of the catalyst increases with the increase of cerium oxide loading. Therefore, changing the cerium oxide loading can adjust the basicity strength and number of basic centers of the solid base catalyst.
[0046] 2. Preparation of solid base supported nickel carbon dioxide hydrogenation catalyst
[0047] Example 6
[0048] Take 1g of the solid base catalyst CeO2 / MMT-1 prepared in Example 1 and place it in a 250ml beaker, add 50ml of water and stir at room temperature for 4 hours to obtain a fully hydrated solid base catalyst aqueous solution. Take 80ml of 0.016mol / L nickel nitrate solution and 80ml of 0.032mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. The obtained nickel nitrate solution and sodium hydroxide solution ice cubes are added to the above-mentioned solid base catalyst aqueous solution stirred by a magnetic stirrer in a way that they melt and release at room temperature, stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 100°C for 12 hours, pass hydrogen at 550°C for 4 hours, cool to room temperature under a hydrogen atmosphere, and then pass O2 / N2 at room temperature. The mixed gas passivation of 0.5-1.0% by volume ratio is passed for 4 hours to obtain a solid base supported metal nickel carbon dioxide hydrogenation catalyst that can be directly stored in the air, represented by Ni-CeO2 / MMT-1.
[0049] Example 7
[0050] Take 1g of the solid base catalyst CeO2 / MMT-2 prepared in Example 2 and place it in a 500ml beaker, add 50ml of water and stir at room temperature for 4 hours to obtain a fully hydrated solid base catalyst aqueous solution. Take 160ml of 0.008mol / L nickel nitrate solution and 160ml of 0.016mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. The obtained nickel nitrate solution and sodium hydroxide solution ice cubes are added to the above-mentioned solid base catalyst aqueous solution stirred by a magnetic stirrer in a way that they melt and release at room temperature, stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 100°C for 12 hours, pass hydrogen at 550°C for 4 hours, cool to room temperature under a hydrogen atmosphere, then pass O2 / N2 at room temperature with a mixed gas passivation of 0.5-1.0% by volume for 4 hours to obtain a solid base supported metal nickel carbon dioxide hydrogenation catalyst that can be directly stored in the air, represented by Ni-CeO2 / MMT-2.
[0051] Example 8
[0052] Take 1g of the solid base catalyst CeO2 / MMT-3 prepared in Example 3 and place it in a 250ml beaker, add 50ml of water and stir at room temperature for 4 hours to obtain a fully hydrated solid base catalyst aqueous solution. Take 32ml of 0.040mol / L nickel nitrate solution and 32ml of 0.080mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. The obtained nickel nitrate solution and sodium hydroxide solution ice cubes are added to the above-mentioned solid base catalyst aqueous solution stirred by a magnetic stirrer in a way that they melt and release at room temperature, stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 100°C for 12 hours, pass hydrogen at 550°C for 4 hours, cool to room temperature under a hydrogen atmosphere, and then pass O2 / N2 at room temperature. The mixed gas passivation with a volume ratio of 0.5-1.0% for 4 hours obtains a solid base supported metal nickel carbon dioxide hydrogenation catalyst that can be directly stored in the air, represented by Ni-CeO2 / MMT-3.
[0053] Example 9
[0054] Take 1g of the solid base catalyst CeO2 / MMT-4 prepared in Example 4 and place it in a 250ml beaker, add 50ml of water and stir at room temperature for 4 hours to obtain a fully hydrated solid base catalyst aqueous solution. Take 80ml of 0.016mol / L nickel nitrate solution and 80ml of 0.032mol / L sodium hydroxide solution respectively, and freeze them into ice cubes. The obtained nickel nitrate solution and sodium hydroxide solution ice cubes are added to the above-mentioned solid base catalyst aqueous solution stirred by a magnetic stirrer in a way that they melt and release at room temperature, stir and react while melting until the ice cubes are completely melted, centrifuge and wash 3 times, dry at 100°C for 12 hours, pass hydrogen at 550°C for 4 hours, cool to room temperature under a hydrogen atmosphere, and then pass O2 / N2 at room temperature. The mixed gas passivation of the volume ratio of 0.5-1.0% for 4 hours obtains a solid base supported metal nickel carbon dioxide hydrogenation catalyst that can be directly stored in the air, represented by Ni-CeO2 / MMT-4.
[0055] The Ni-CeO2 / MMT-4 catalyst was characterized by XRD. The XRD test was carried out on a D8 Advance polycrystalline X-ray diffractometer produced by Bruker AXS, Germany. The results are shown in Figure 2 It can be found from the figure that in addition to the characteristic diffraction peaks of montmorillonite (2θ=35.1°, 62.0°, 73.3°), characteristic peaks of cerium oxide were observed at 2θ=47.2° and 55.2°, and characteristic peaks of metallic nickel were observed at 2θ=44.4° and 76.5°, which shows that cerium oxide and metallic nickel are loaded on the montmorillonite carrier without destroying the montmorillonite structure, and a solid base-loaded nickel carbon dioxide methanation catalyst was successfully prepared.
[0056] Comparative Example 1
[0057] Except that sodium-montmorillonite was used to replace CeO2 / MMT-1, the other steps were the same as those in Example 6 to prepare a montmorillonite-supported nickel-carbon dioxide hydrogenation catalyst, denoted by Ni / MMT.
[0058] III. Activity Evaluation of the Solid Base Supported Metal Nickel Carbon Dioxide Hydrogenation Catalyst of the Present Invention
[0059] Example 10
[0060] Evaluation of carbon dioxide hydrogenation activity of Ni-CeO2 / MMT-1 catalyst supported by solid base: The evaluation of carbon dioxide hydrogenation performance of Ni-CeO2 / MMT-1 catalyst was carried out on a micro fixed bed reactor. The specific operation steps and reaction conditions are as follows: 0.25g Ni-CeO2 / MMT-1 catalyst was added to the fixed bed reactor, and the catalyst was activated by passing H2 at 300℃ for 2 hours, then cooled to the reaction temperature of 180℃, and H2+CO2 reaction gas (H2:CO2=1:4) was passed to react at 0.25MPa, and the hydrogenation product was sampled and analyzed online by GC-1690 gas chromatograph using the internal standard method.
[0061] The evaluation of carbon dioxide hydrogenation and methanation activity of Ni-CeO2 / MMT-2, Ni-CeO2 / MMT-3, Ni-CeO2 / MMT-4 and Ni / MMT catalysts was the same as that of Ni-CeO2 / MMT-1 catalyst, and the reaction results are shown in Table 1.
[0062] Table 1 Carbon dioxide methanation performance at 180℃ over solid base supported nickel catalysts with different CeO2 loadings
[0063]
[0064] Reaction conditions: space velocity 20000h -1 , 0.25g catalyst, 0.25MPa CO2+H2 (CO2:H2=1:4)
[0065] The results in Table 1 show that the solid base catalyst prepared by the present invention has excellent carbon dioxide hydrogenation performance. According to the reaction results, the carbon dioxide conversion rate of the Ni / MMT catalyst at a reaction temperature of 180°C is 13.2%. Compared with it, the Ni-CeO2 / MMT-1 catalyst is relatively increased by 20%; the Ni-CeO2 / MMT-2 catalyst is relatively increased by 148%; the Ni-CeO2 / MMT-3 catalyst is relatively increased by 130%; and the Ni-CeO2 / MMT-4 is relatively increased by 56%. The activity of the solid base carbon dioxide hydrogenation catalyst with different cerium oxide loadings prepared in the present invention is higher than that of the Ni / MMT catalyst, among which the CeO2 / MMT-2 catalyst has the best activity, with a conversion rate of 32.7% and a methane selectivity of 100%. At the same time, the solid base catalyst provided by the present invention has the advantages of simple and convenient preparation, cheap and easy-to-obtain carriers, and is conducive to industrial production. Its adjustable alkalinity also greatly broadens the application field of the solid base catalyst.
Claims
1. A method for preparing a carbon dioxide hydrogenation catalyst, Features The steps include: (1) Mixing montmorillonite and water in a mass ratio of 1:50-100, stirring at room temperature for 2-4 hours to obtain a fully hydrated montmorillonite aqueous solution; (2) freezing a cerium metal salt solution having a mass ratio of metal salt to montmorillonite of 2.5 to 10:100 and a concentration of 0.001 to 0.008 mol / L, and a hydroxide solution having a molar ratio of 2 to 3:1 to cerium salt and a concentration of 0.002 to 0.024 mol / L into ice cubes; (3) adding the metal salt solution and hydroxide solution ice cubes obtained in step (2) to the montmorillonite aqueous solution obtained in step (1) in a manner of melting and releasing at room temperature, stirring while melting until the ice cubes are completely melted, centrifuging and washing three times, and drying at 80-100° C. for 8-16 hours to obtain a solid base catalyst precursor; (4) calcining the solid base catalyst precursor obtained in step (3) at 450-550° C. in an air atmosphere for 3-6 hours, and cooling to room temperature to obtain a solid base catalyst; (5) mixing the solid base catalyst prepared in step (4) with water at a mass ratio of 1:100, and stirring at room temperature for 4 h to obtain a fully hydrated solid base catalyst aqueous solution; (6) freezing a nickel nitrate solution having a concentration of 0.008 to 0.040 mol / L and a sodium hydroxide solution having a molar ratio of 2:1 to nickel nitrate and a concentration of 0.016 to 0.080 mol / L into ice cubes; (7) adding the nickel nitrate solution and sodium hydroxide solution ice cubes obtained in step (6) to the solid base catalyst aqueous solution obtained in step (5) in a manner of melting and releasing at room temperature, stirring while melting until the ice cubes are completely melted, centrifuging and washing three times, and drying at 100° C. for 12 hours to obtain a solid base-supported nickel hydroxide methane hydrogenation catalyst precursor; (8) The solid base supported nickel hydroxide methane hydrogenation catalyst precursor obtained in step (7) was reduced by passing hydrogen at 550°C for 4 hours, cooled to room temperature under a hydrogen atmosphere, and then passed oxygen at room temperature. 2 / N 2 The mixed gas with a volume ratio of 0.5 to 1.0% was passivated for 4 hours to obtain a carbon dioxide hydrogenation catalyst that can be directly stored in the air.
2. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, It is characterized in that The montmorillonite in step (1) is sodium montmorillonite.
3. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, It is characterized in that The cerium salt in step (2) is any one of cerium nitrate, cerium chloride and cerium sulfate.
4. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 3, It is characterized in that The cerium salt in step (2) is cerium nitrate.
5. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 1, It is characterized in that The hydroxide in step (2) is sodium hydroxide or potassium hydroxide.
6. The method for preparing the carbon dioxide hydrogenation catalyst according to claim 5, It is characterized in that The hydroxide in step (2) is sodium hydroxide.
7. A carbon dioxide hydrogenation catalyst prepared by the method as claimed in claim 1.
8. Use of the carbon dioxide hydrogenation catalyst as claimed in claim 7 in carbon dioxide hydrogenation reaction.