A metal core welding wire with high crack resistance for GH3030 high temperature alloy
By using 80%Ni-20%Cr nickel-based alloy tape and multi-component flux-core welding wire in GH3030 high-temperature alloy welding, the problem of thermal cracks and performance degradation of welding joints is solved, and the high thermal crack resistance of welding joints is achieved. High temperature mechanical properties improve, extend service life and simplify welding process.
Patent Information
- Application Number
- CN202211555123.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-05
AI Technical Summary
GH3030 high-temperature alloy is prone to thermal cracks during welding, and traditional welding materials cause the mechanical properties and corrosion resistance of the welded joints to decrease, increasing the difficulty of welding and repair workload.
Drugs using 80%Ni-20%Cr nickel-based alloy tape as the coating layer, and the powder core is added with metal chromium, ferroniobium, electrolytic manganese metal, aluminum-magnesium alloy, 45# ferrosilicon, calcium fluoride and rare earth cerium. The core welding wire forms a stable deposited metal structure through appropriate powder particle size and welding parameters to improve the thermal crack resistance and high temperature mechanical properties of the welded joints.
It significantly improves the thermal crack resistance and high temperature mechanical properties of GH3030 high-temperature alloy welded joints, extends the service life, reduces the pre-weld cleaning steps, and reduces the post-weld repair workload.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flux-cored welding wires, and in particular relates to a flux-cored welding wire for welding GH3030 high-temperature alloy, which is mainly used for connection and surfacing of GH3030 high-temperature alloy. Background Art
[0002] From 1956 to the early 1970s, the first batch of high-temperature alloy GH3030 was successfully tested in my country, marking the beginning of my country's high-temperature alloy. GH3030 is a solid solution strengthened nickel-based high-temperature alloy with good structural stability, high high-temperature strength, good oxidation resistance and heat corrosion resistance, good fatigue resistance, fracture toughness and other comprehensive properties. GH3030 high-temperature alloy can work for a long time under high-speed dynamic loads and high-temperature strengthening atmosphere or gas conditions, and is widely used in aerospace, atomic energy, locomotives and petrochemical industries.
[0003] Due to the high nickel content in GH3030, during the welding process, nickel easily forms a low melting point eutectic with impurity elements such as P, S, Pb, Bi, etc., which is very easy to produce welding hot cracks. The microstructure of GH3030 is a single austenite. During the welding process, the grains in the welded joint are easy to grow. Under the action of external load or under the condition of large restraint, the welded joint is prone to cracking.
[0004] The current welding methods for GH3030 high temperature alloy mainly include laser welding, argon arc welding, brazing, inert gas shielded welding and other welding methods. The welding materials used for GH3030 high temperature alloy mainly include HGH3030 high temperature alloy cold drawing wire, and its model is TT-82. The chemical composition of HGH3030 cold drawing wire is basically the same as that of GH3030.
[0005] When laser welding GH3030 high temperature alloy, it is usually self-melting welding, and no filler material is used. When laser self-melting welding GH3030, due to the evaporation of alloying elements, the strength of the welded joint is usually lower than the strength of the parent material. Laser welding can also use powder materials to weld GH3030 high temperature alloy, but the assembly clearance requirements of the welded joint are very strict, and high requirements are placed on the fixture, which increases the workload. On the other hand, due to the high price of laser welding powder and the low powder utilization rate, it is currently only suitable for surfacing of precision parts. In addition, laser welding is not suitable for the base weld of the welded joint. Due to the high price and high maintenance cost of laser welding equipment, its application is subject to certain restrictions.
[0006] When GH3030 high temperature alloy is welded by argon arc welding or inert gas shielded welding (MIG), the welding material used is HGH3030 solid welding wire, whose chemical composition is basically the same as that of the parent material. When HGH3030 welding wire is used to weld GH3030, its chemical composition is close to that of GH3030. During welding, due to the burning of alloy elements, the alloy element content in the weld is slightly lower than that of the parent material, especially the Ti element in HGH3030 welding wire is seriously burned, which not only reduces the mechanical properties of the welded joint, but also reduces the corrosion resistance of the welded joint. The welded joint is usually low-strength matching.
[0007] On the other hand, since the deposited metal structure of HGH3030 welding wire and the structure of GH3030 are both single-phase austenite structures, hot cracks are very likely to occur during the welding process. In addition, since the nickel content in HGH3030 welding wire and GH3030 base material reaches more than 60%, nickel can form a low-melting point eutectic with impurity elements such as P and S in the welding material and base material, further increasing the tendency of hot cracks. When using argon arc welding or inert gas shielded welding, when the restraint is large or the overlay is large, welding hot cracks are very likely to occur, which will lead to the failure of the structural parts or greatly increase the workload of post-weld repair.
[0008] During the welding process, no matter which welding method is used, since nickel is easy to form a low-melting point eutectic with impurity elements such as S and P, when welding GH3030 high-temperature alloy, the dirt inside and on both sides of the welding groove must be strictly cleaned, and acetone must be used for cleaning when necessary, which reduces labor efficiency. Summary of the invention
[0009] In order to overcome the shortcomings of the prior art, the present invention develops a GH3030 high-temperature alloy flux-cored welding wire, which has good thermal crack resistance and does not require acetone to clean the weld and the base material on both sides of the groove during the welding process.
[0010] A high-crack-resistant GH3030 high-temperature alloy metal core welding wire, characterized in that a commonly used 80% Ni-20Cr nickel-based alloy strip is used as a coating layer, and the mass percentages of the alloy components in the powder core are as follows: the mass percentage of metal chromium powder is 20-34%, the mass percentage of ferroniobium (60% Nb) powder is 1-2.5%, the content of electrolytic manganese is 1-3.5%, the mass percentage of aluminum-magnesium alloy powder is 1-3%, the mass percentage of 45# ferrosilicon is 1-4%, the mass percentage of calcium fluoride is 2-4%, the mass percentage of rare earth cerium is 2-5%, and the balance is nickel powder; the particle size of the rare earth cerium powder is 200 mesh, and the particle sizes of the remaining powders are all 80 mesh.
[0011] The present invention adopts 20% Cr-80Ni nickel-based alloy strip, which has a width of 10mm and a thickness range of 0.3-0.5mm. The filling rate of the metal core welding wire of the present invention is 23-30%, and the diameter range of the welding wire is 1.2-2.5. The current range of the welding wire during welding is 80A-260A, and the welding voltage range is 22V-33V; the welding shielding gas is pure argon or mixed gas (80% Ar+20% CO 2 ), gas flow rate is 10-25L / min.
[0012] The chemical composition range of the deposited metal of the flux-cored welding wire made of 20% Cr-80Ni nickel-based alloy strip is as follows (mass percentage):
[0013] C: ≤0.12%, Si: ≤0.8%, Mn: ≤0.7%, S≤0.020, P≤0.030, Cr: 19-22%, Nb: 0.15-0.35%, Al: ≤0.15%, Fe: ≤1.5%, Re: 0.02-0.08%, Ni: balance.
[0014] The components and functions of the flux-cored welding wire of the present invention are as follows:
[0015] Metal chromium powder: plays the role of alloying, improving the hardness and strength of the welded joint. Its main function is to improve the oxidation resistance and corrosion resistance of steel, and ensure that the weld has higher mechanical properties at room temperature and high temperature.
[0016] Metal nickel powder: plays the role of alloying, stabilizes and promotes austenite formation elements, improves the stability of austenite, improves the high temperature strength, creep resistance and high temperature resistance of steel, and ensures that the weld has higher mechanical properties at room temperature and high temperature.
[0017] Niobium iron: Improves the high temperature resistance and corrosion resistance of steel.
[0018] Electrolytic Manganese Metal: Deoxidation, desulfurization, and improving the strength of welded joints.
[0019] Aluminum-magnesium alloy powder: Improves the heat resistance and corrosion resistance of steel. Can deoxidize during welding.
[0020] Ferrosilicon No. 45: deoxidizes; accelerates the melting of welding wire; improves the heat resistance of steel.
[0021] Calcium fluoride: Desulfurization; can be used as a strong diluent to facilitate the escape of hydrogen from the weld.
[0022] Rare earth cerium: deoxidation, desulfurization, improving impact toughness; improving the oxidation resistance and corrosion resistance of steel. Improve the fluidity of the weld, reduce impurities and pore sensitivity in the weld; refine the grain; improve high temperature strength.
[0023] Technical problems solved by the present invention and beneficial effects achieved
[0024] The present invention develops a metal core welding wire for welding GH3030 high temperature alloy. When the present invention is used to weld the GH3030 high temperature alloy, the welded joint has excellent thermal crack resistance and high temperature mechanical properties.
[0025] When the traditional HGH3030 solid welding wire is used to weld the GH3030 high-temperature alloy, the Ti element in the welding wire is easily burned during the welding process, which reduces the room temperature mechanical properties, high temperature mechanical properties and corrosion resistance of the welded joint, and greatly reduces the service life of the GH3030 high-temperature alloy welding structure or cladding layer. The present invention adds an appropriate amount of ferroniobium to the welding wire. During the welding process, Nb and C can form a stable compound, which is dispersed in the weld. On the one hand, it can refine the grains and reduce the tendency of hot cracks. At the same time, it avoids the problem of reduced performance of the welded joint caused by the use of HGH3030 solid welding wire. On the other hand, the addition of niobium improves the mechanical properties and high-temperature creep strength of the welded joint, which is beneficial to improving the service life of the GH3030 high-temperature alloy under high temperature conditions.
[0026] In traditional solid welding wires such as HGH3030, the weld structure is single-phase austenite. During the welding process, the austenite grains will inevitably grow seriously under the action of heat, and thermal cracks are very likely to occur when welding under restrained conditions. In the present invention, by adding an appropriate amount of ferroniobium to the welding wire, a niobium-containing compound is formed. During the solidification process of the weld, the niobium compound first crystallizes out from the liquid metal, and after the weld is completely solidified, it is pinned to the boundary of the austenite grains, thereby inhibiting the growth of the austenite grains and reducing the tendency of thermal cracking.
[0027] On the other hand, although the sulfur and phosphorus content in the HGH3030 solid welding wire is controlled, thermal cracks often occur in actual welding, especially at the arc closing point. In the GH3030 high-temperature alloy welding structure with a large degree of restraint, even longitudinal cracks are generated. In addition, when the GH3030 high-temperature alloy is connected and welded, the groove and the parent materials on both sides must be strictly cleaned, and acetone must be used for cleaning when necessary, which increases the workload before welding. If the groove is not cleaned, the dirt on the groove or the surface of the welding wire will also enter the weld, further increasing the crack sensitivity of the welded joint. In the present invention, an appropriate amount of rare earth cerium is added to the welding wire, which can purify sulfur and other impurity elements in the weld and improve the crack resistance of the welded joint. In addition, the addition of rare earth cerium further improves the high-temperature oxidation resistance of the GH3030 high-temperature alloy welded joint and the high-temperature mechanical properties of the welded joint. DETAILED DESCRIPTION
[0028] The welding wire of the present invention is manufactured by using a conventional flux-cored welding wire production line. The steel strip is first rolled into a U-shape, the prepared powder is added into the groove of the U-shaped steel strip, and then the U-shaped groove is closed to wrap the powder therein.
[0029] The metal core welding wire of the present invention is selected for specific implementation. The welding base material is selected as GH3030 high temperature alloy. The welding joint sample is selected according to GB / T2651-2008. The specific embodiment is as follows:
[0030] Embodiment 1: A 10×0.5 (10 mm in width and 0.5 mm in thickness) Ni80Cr20 nickel strip is selected with a filling rate of 23%. After drawing and reducing the diameter, a welding wire with a diameter of 1.2 mm is obtained.
[0031] The mass percentage of each alloy component in the powder core is:
[0032] The mass percentage of metallic chromium is 34%; the mass percentage of ferroniobium is 2.5%; the mass percentage of electrolytic metallic manganese is 3.5%; the mass percentage of aluminum-magnesium alloy powder is 2%; the mass percentage of No. 45 ferrosilicon is 4%; the mass percentage of calcium fluoride is 2%; the mass percentage of rare earth cerium is 5%; and the balance is nickel powder.
[0033] The welding process parameters are as follows: welding current is 160A, welding voltage is 26V, welding shielding gas is pure argon gas, shielding gas flow rate is 10L / min, and welding method is argon arc welding with molten inert gas.
[0034] Example 2: A 10×0.5 (10 mm wide, 0.5 mm thick) Ni80Cr20 nickel strip is selected with a filling rate of 24%. After drawing and reducing the diameter, a welding wire with a diameter of 1.2 mm is obtained.
[0035] The mass percentage of each alloy component in the powder core is:
[0036] The mass percentage of metallic chromium is 33%; the mass percentage of ferroniobium is 2%; the mass percentage of electrolytic metallic manganese is 3%; the mass percentage of aluminum-magnesium alloy powder is 1%; the mass percentage of No. 45 ferrosilicon is 1%; the mass percentage of calcium fluoride is 4%; the mass percentage of rare earth cerium is 4%; and the balance is nickel powder.
[0037] The welding process parameters are as follows: welding current is 200A, welding voltage is 30V, welding shielding gas is 80%Ar+20%CO 2 , the protective gas flow rate is 15L / min. The welding method is mixed gas shielded welding.
[0038] Embodiment 3: A 10×0.4 (10 mm in width and 0.4 mm in thickness) Ni80Cr20 nickel strip is selected with a filling rate of 25%. After drawing and reducing the diameter, a welding wire with a diameter of 1.6 mm is obtained.
[0039] The mass percentage of each alloy component in the powder core is:
[0040] The mass percentage of metallic chromium is 30%; the mass percentage of ferroniobium is 2%; the mass percentage of electrolytic metallic manganese is 2%; the mass percentage of aluminum-magnesium alloy powder is 3%; the mass percentage of No. 45 ferrosilicon is 2%; the mass percentage of calcium fluoride is 3%; the mass percentage of rare earth cerium is 4%; and the balance is nickel powder.
[0041] The welding process parameters are as follows: welding current is 260A, welding voltage is 33V, welding shielding gas is 80%Ar+20%CO 2 , the protective gas flow rate is 15L / min. The welding method is mixed gas shielded welding.
[0042] Example 4: A 10×0.4 (10 mm wide, 0.4 mm thick) Ni80Cr20 nickel strip is selected with a filling rate of 26%. After drawing and reducing the diameter, a welding wire with a diameter of 1.6 mm is obtained.
[0043] The mass percentage of each alloy component in the powder core is:
[0044] The mass percentage of metallic chromium is 28%; the mass percentage of ferroniobium is 2%; the mass percentage of electrolytic metallic manganese is 2%; the mass percentage of aluminum-magnesium alloy powder is 2%; the mass percentage of No. 45 ferrosilicon is 2%; the mass percentage of calcium fluoride is 3%; the mass percentage of rare earth cerium is 4%; and the balance is nickel powder.
[0045] The welding process parameters are as follows: welding current is 260A, welding voltage is 32V, welding shielding gas is 80%Ar+20%CO 2 , the protective gas flow rate is 15L / min. The welding method is mixed gas shielded welding.
[0046] Example 5: A 10×0.4 (10 mm wide, 0.4 mm thick) Ni80Cr20 nickel strip is selected with a filling rate of 26%. After drawing and reducing the diameter, a welding wire with a diameter of 2.0 mm is obtained.
[0047] The mass percentage of each alloy component in the powder core is:
[0048] The mass percentage of metallic chromium is 26%; the mass percentage of ferroniobium is 2%; the mass percentage of electrolytic metallic manganese is 1%; the mass percentage of aluminum-magnesium alloy powder is 2%; the mass percentage of No. 45 ferrosilicon is 2%; the mass percentage of calcium fluoride is 3%; the mass percentage of rare earth cerium is 4%; and the balance is nickel powder.
[0049] The welding process parameters are as follows: welding current is 80A, welding voltage is 22V, welding shielding gas is pure argon gas, shielding gas flow rate is 20L / min, and welding method is argon arc welding.
[0050] Example 6: A 10×0.3 (10 mm wide, 0.3 mm thick) Ni80Cr20 nickel strip is selected with a filling rate of 30%. After drawing and reducing the diameter, a welding wire with a diameter of 2.5 mm is obtained.
[0051] The mass percentage of each alloy component in the powder core is:
[0052] The mass percentage of metallic chromium is 20%; the mass percentage of ferroniobium is 1%; the mass percentage of electrolytic metallic manganese is 1%; the mass percentage of aluminum-magnesium alloy powder is 1%; the mass percentage of No. 45 ferrosilicon is 2%; the mass percentage of calcium fluoride is 2%; the mass percentage of rare earth cerium is 2%; and the balance is nickel powder.
[0053] The welding process parameters are as follows: welding current is 200A, welding voltage is 22V, welding shielding gas is pure argon gas, shielding gas flow rate is 25L / min, and welding method is argon arc welding.
[0054] VII. Comparative Example and the present invention compared test results
[0055] Comparative tests were conducted using the present invention and comparative welding materials. The comparative welding material selected HGH3030 (TT-82) cold-drawn wire, the wire diameter was 2mm, the welding current was 160A, and the welding voltage was 24V. Argon arc welding was used as the welding method. The chemical composition of the deposited metal and the mechanical properties of the welded joint of the two welding materials were compared. The thickness of the GH3030 high-temperature alloy base plate was 10mm, the groove angle was 60 degrees, the groove gap was 3mm, and no groove blunt edge was left. After welding, the chemical composition of the deposited metal and the tensile strength of the welded joint were tested. The chemical composition of the deposited metal was tested in accordance with GB / T25777-2010. The mechanical properties of the welded joint were tested in accordance with GB / T2651-2008. The chemical composition of the deposited metal is shown in Table 1. The test results of the mechanical properties of the welded joint are shown in Table 2. After the arc crater crack appears during the welding of the comparative wire HGH3030 (TT-82), it needs to be repaired in time until there is no crack. The welded joints welded by the welding materials of the present invention and the comparative welding materials are required to be inspected. After the inspection shows no defects, the mechanical properties test and high-temperature tensile strength test are carried out on the welded joints. The experimental results show that the tensile strength of the deposited metal welded by HGH3030 cold-drawn wire is only about 92% of the tensile strength of the base material (681MPa). The welded joints welded by the welding wire of the present invention all exceed the tensile strength of the base material itself. It can be seen from Table 2 that the elongation of the welding wire of the present invention is higher than the elongation of the comparative welding wire. By comparing the tensile strength of the two welding materials under high temperature conditions of 700°C, it can be seen that the high-temperature tensile strength of the HGH3030 cold-drawn wire is less than 200MPa, and the welding wire of the present invention is higher than 260MPa, indicating that the welding wire of the present invention has better high-temperature mechanical properties.
[0056] Table 1 Chemical composition of deposited metal
[0057] Example C Si Mn S P Cr Fe Ti Nb Ce Ni Comparative Example 0.04 0.2 0.45 0.015 0.022 19.3 1.3 0.07 -- -- margin Example 1 0.027 0.33 0.65 0.001 0.011 21.80 1.1 -- 0.34 0.10 margin Example 2 0.026 0.12 0.65 0.002 0.011 20.80 1.0 -- 0.29 0.08 margin Example 3 0.025 0.19 0.58 0.002 0.012 20.46 1.2 -- 0.30 0.07 margin Example 4 0.026 0.20 0.60 0.001 0.011 20.05 0.9 -- 0.31 0.07 margin Example 5 0.020 0.19 0.42 0.001 0.011 19.60 0.8 -- 0.35 0.08 margin Example 6 0.021 0.20 0.43 0.001 0.011 19.16 1.0 -- 0.18 0.05 margin
[0058] Table 2 Mechanical properties of welded joints at room temperature
[0059]
Claims
1. A metal core welding wire for GH3030 high temperature alloy, characterized in that: A commonly used 80% Ni-20% Cr alloy strip is used as the coating layer; the mass percentages of the alloy components in the powder core are as follows: the mass percentage of metal chromium powder is 20-34%, the mass percentage of ferroniobium powder is 1-2.5%, the content of electrolytic metal manganese is 1-3.5%, the mass percentage of aluminum-magnesium alloy powder is 1-3%, the mass percentage of 45# ferrosilicon is 1-4%, the mass percentage of calcium fluoride is 2-4%, the mass percentage of rare earth cerium is 2-5%, and the balance is nickel powder; the powder particle size of rare earth cerium is 200 mesh, and the particle sizes of the other powders are all 80 mesh; the filling rate of the metal core welding wire is 23-30%, wherein the ferroniobium contains 60% Nb.
2. A metal core welding wire for GH3030 high temperature alloy according to claim 1, characterized in that: The diameter of the welding wire ranges from 1.2-2.5mm.
3. A metal core welding wire for GH3030 high temperature alloy according to claim 1, characterized in that: For TIG, MIG and MAG welding.
4. A metal core welding wire for GH3030 high temperature alloy according to claim 1, characterized in that: The chemical composition of the deposited metal is as follows according to the mass percentage range: C: ≤0.12%, Si: ≤0.8%, Mn: ≤0.7%, S ≤0.020, P≤0.030, Cr: 19-22%, Nb: 0.15-0.35%, Al: ≤0.15%, Fe: ≤1.5%, RE: 0.02-0.08%, Ni: balance.
5. Use of the metal core welding wire for GH3030 high temperature alloy according to claim 1 for welding GH3030 high temperature alloy.
Citation Information
Cited By
Matched welding wire for nickel-based heat-resistant alloy C-HRA-3 and preparation method and application of matched welding wire
CN121179075A