A coating of welding rod for nuclear power plant internal components, welding rod and preparation method thereof

By using specific ingredients and contents of the powdered skin in the welding rod, the alkaline slag system and ferrite are formed, and combined with the functions of rare earths and aluminum-zirconium alloys, the problem of insufficient strength and toughness in the components of the nuclear power plant stack is solved. High strength and toughness are achieved.

CN115922151BActive Publication Date: 2024-11-12ATLANTIC CHINA WELDING CONSUMABLES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211584878.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-12
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Existing welding rods are difficult to meet the high strength and toughness requirements of the components in the nuclear power plant stack, especially in the welded state and the heat-treated state, the room temperature impact function is insufficient.

Method used

Using a coating of welding rod for components of nuclear power plant rechargeable components, including marble, fluorite, rutile, microcarbon ferrochromium, metal nickel, ferromolybdenum, iron niobium, rare earth and aluminum-zirconium alloy, etc., to control the The content and particle size form alkaline slag system and ferrite, improve the molding and corrosion resistance of the weld, and refine the grains through the action of rare earths and aluminum-zirconium alloys to enhance the strength and toughness of the weld.

Benefits of technology

It realizes high strength and high toughness of welding rods in welding and heat-treatment states, meets the high strength and high toughness requirements of the components in the nuclear power plant stack, and improves room temperature impact work and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115922151B_ABST
    Figure CN115922151B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of nuclear power welding materials, and in particular to a coating, welding rod and preparation method of a welding rod for a nuclear power plant internal component; the raw materials of the coating include: marble, fluorite, rutile, wollastonite, micro-carbon ferrochrome, metallic nickel, electrolytic manganese, ferromolybdenum, ferroniobium, aluminum-zirconium alloy, rare earth, soda ash and sodium alginate; the method includes: mixing the raw materials of the coating described in the first aspect to obtain a coating powder; adding a binder to the coating powder to obtain a mixed powder; coating the mixed powder on the surface of the welding core, and baking it in steps to obtain a welding rod; by controlling the content of marble, fluorite, rutile, micro-carbon ferrochrome, ferromolybdenum, ferroniobium, soda ash and sodium alginate in the coating, and introducing rare earth elements and aluminum-zirconium alloy, utilizing the interaction between rare earth elements and aluminum-zirconium alloy, and through the designed coating composition, the high-strength and high-toughness welding requirements required for the nuclear power plant internal component can be comprehensively obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nuclear power welding materials, and in particular to a coating, welding rod and preparation method of a welding rod for a nuclear power plant internal component. Background Art

[0002] AP1000 nuclear power technology is an advanced passive pressurized water reactor nuclear power technology and the safest and most advanced commercial nuclear power technology in the global nuclear power market. Among them, the nuclear power plant is the key to AP1000 nuclear power technology. Currently, the nuclear power plant uses nuclear fuel instead of ordinary fuel, and uses the fission reaction of the nuclear fuel in the nuclear reactor to generate heat energy and convert it into power.

[0003] With the development of nuclear power technology and the requirements for special equipment manufacturing, the high performance and domestic application of welding materials for supporting the internal components of nuclear power plants are imminent. Since nuclear power plants are generally composed of multiple internal components by welding, there are no special welding rods for the internal components of nuclear power plants. At present, there are welding rods for welding key parts of stainless steel nuclear power fields with high requirements for corrosion resistance and high temperature resistance, but their mechanical properties are: the mechanical properties of the deposited metal at room temperature in the welded state: Rm = 564MPa, Rp0.2 = 403MPa, A = 44%, and the impact energy KV2 values ​​at room temperature are: 84J, 8 5J, 87J; high temperature 360℃ mechanical properties: Rm=415MPa, Rp0.2=302MPa; mechanical properties of deposited metal at room temperature after 610℃×40h heat treatment: Rm=593MPa, Rp0.2=390MPa, A=46%, and the impact energy KV2 values ​​at room temperature are: 80J, 82J, 78J respectively; high temperature 360℃ mechanical properties: Rm=412MPa, Rp0.2=291MPa; It can be seen from the mechanical property data that the room temperature impact energy of the welding rod in the welded state and the heat treated state does not meet the special requirements of high strength and high toughness of the internal components of the nuclear power plant.

[0004] Therefore, how to provide a coating for welding rods for nuclear power plant internal components to meet the requirements of high strength and high toughness of nuclear power plant internal components is a technical problem that urgently needs to be solved. Summary of the invention

[0005] The present application provides a coating, welding rod and preparation method of a welding rod for a nuclear power plant internal component, so as to solve the technical problem that the welding rod in the prior art is difficult to meet the requirements of high strength and high toughness of the nuclear power plant internal component.

[0006] In the first aspect, the present application provides a coating for welding rods for internal components of a nuclear power plant. The raw materials of the coating include, by weight: marble: 19.0 to 23.0 parts, fluorite: 22.0 to 26.0 parts, rutile: 4.0 to 6.0 parts, wollastonite: 7.0 to 9.0 parts, micro-carbon ferrochrome: 13.5 to 16.5 parts, metallic nickel: 4.5 to 5.5 parts, electrolytic manganese: 2.5 to 3.5 parts, ferromolybdenum: 0.8 to 1.2 parts, ferroniobium: 0.2 to 0.4 parts, aluminum-zirconium alloy: 1.0 to 3.0 parts, rare earth: 2.0 to 3.0 parts, soda ash: 1.0 to 1.4 parts, and sodium alginate: 2.2 to 2.6 parts.

[0007] Optionally, based on the total weight of the marble, the particle size of the marble satisfies: 80 mesh ≥ 65 weight %; and / or,

[0008] Based on the total weight of the fluorite, the particle size of the fluorite satisfies: 50 mesh ≥ 96 weight %; and / or,

[0009] Based on the total weight of the rutile, the particle size of the rutile satisfies: 40 mesh ≥ 97 weight %; and / or,

[0010] Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 100 mesh ≥ 90 weight %; and / or,

[0011] Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome satisfies: 40 mesh ≥ 98 weight %; and / or,

[0012] Based on the total weight of the metallic nickel, the particle size of the metallic nickel satisfies: 60 mesh ≥ 95 weight %; and / or,

[0013] Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese satisfies: 40 mesh ≥ 98 weight %; and / or,

[0014] Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum satisfies: 40 mesh ≥ 98 weight %; and / or,

[0015] Based on the total weight of the ferroniobium, the particle size of the ferroniobium satisfies: 50 mesh ≥ 96 weight %; and / or,

[0016] Based on the total weight of the aluminum-zirconium alloy, the particle size of the aluminum-zirconium alloy satisfies: 60 mesh ≥ 97 weight %; and / or,

[0017] Based on the total weight of the rare earth, the particle size of the rare earth satisfies: 80 mesh ≥ 95 weight %; and / or,

[0018] Based on the total weight of the soda ash, the particle size of the soda ash satisfies: 80 mesh ≥ 98 weight %; and / or,

[0019] Based on the total weight of the sodium alginate, the particle size of the sodium alginate satisfies: 140 mesh ≥ 97 weight %.

[0020] Optionally, based on the total weight of the marble, the particle size of the marble satisfies: 50 mesh ≥ 96 weight %; and / or,

[0021] Based on the total weight of the fluorite, the particle size of the fluorite is 30 mesh; and / or,

[0022] Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 50 mesh ≥ 97 weight %; and / or,

[0023] Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome is 30 mesh; and / or,

[0024] Based on the total weight of the metallic nickel, the particle size of the metallic nickel is 30 mesh; and / or,

[0025] Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese is 30 mesh; and / or,

[0026] Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum is 30 mesh.

[0027] Optionally, based on the total weight of the marble, the CaCO in the marble is 3 The content of ≥96% by weight; and / or,

[0028] Based on the total weight of the fluorite, the CaF 2 The content of ≥96% by weight; and / or,

[0029] Based on the total weight of the rutile, the TiO 2 The content of ≥95.5% by weight; and / or,

[0030] Based on the total weight of the wollastonite, the CaSiO 3 The content of ≥46.0% by weight; and / or,

[0031] Based on the total weight of the low-carbon ferrochrome, the content of Cr in the low-carbon ferrochrome is 65 wt% to 70 wt%; and / or,

[0032] Based on the total weight of the metallic nickel, the content of Ni in the metallic nickel is ≥ 99.5 wt %; and / or,

[0033] Based on the total weight of the electrolytic manganese, the content of Mn in the electrolytic manganese is ≥ 99.5 wt %; and / or,

[0034] Based on the total weight of the ferromolybdenum, the content of Mo in the ferromolybdenum is 55.0 wt% to 60.0 wt%, and the content of Fe in the ferromolybdenum is 40.0 wt% to 45.0 wt%; and / or,

[0035] Based on the total weight of the ferroniobium, the content of Nb in the ferroniobium is 50.0 wt% to 55.0 wt%, and the content of Fe in the ferroniobium is 45.0 wt% to 50.0 wt%; and / or,

[0036] Based on the total weight of the aluminum-zirconium alloy, the content of Al in the aluminum-zirconium alloy is 45.0 wt% to 50.0 wt%, and the content of Zr in the aluminum-zirconium alloy is 49.0 wt% to 51.0 wt%; and / or,

[0037] Based on the total weight of the rare earth, the content of rare earth elements in the rare earth is ≥ 83.0 wt %; and / or,

[0038] Based on the total weight of the soda ash, the Na 2 CO 3 The content of ≥98.5% by weight; and / or,

[0039] Based on the total weight of the sodium alginate, the Na 2 The content of O is 9.5 wt% to 13.0 wt%.

[0040] In a second aspect, the present application provides a welding rod for a nuclear power plant internal component, the welding rod comprising the coating and a welding core as described in the first aspect, the coating coating covering the surface of the welding core.

[0041] Optionally, the chemical composition of the welding core includes, by mass fraction: C≤0.007%, Mn: 1.5%~2.0%, Si≤0.20%, Cr: 21.5%~22.5%, Ni: 11.5%~12.5%, Mo≤0.1%, Cu≤0.05%, N≤0.025%, S≤0.005%, P≤0.010%, Co≤0.010%, V≤0.050%, and the balance is Fe and unavoidable impurities.

[0042] Optionally, the coating and the welding core are bonded by an adhesive, and the adhesive includes a mixture of at least two water glass solutions.

[0043] In a third aspect, the present application provides a method for preparing the welding rod according to the second aspect, the method comprising:

[0044] Mixing the raw materials of the drug coating described in the first aspect to obtain drug coating powder;

[0045] Adding a binder to the coating powder to obtain a mixed powder;

[0046] The mixed powder is coated on the surface of the welding core and baked step by step to obtain a welding rod.

[0047] Optionally, the mass ratio of the binder to the coating powder is 18% to 19%.

[0048] Optionally, the step-by-step baking includes a first baking stage and a second baking stage; the temperature of the first baking stage is 80° C. to 90° C., and the time of the first baking stage is 3.5 h to 4 h; and / or,

[0049] The temperature of the second baking stage is 370° C. to 380° C., and the time of the second baking stage is 2.5 h to 3 h.

[0050] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0051] The embodiment of the present application provides a coating for a welding rod for an in-core component of a nuclear power plant. By controlling the marble content in the coating, the basicity of the slag formed by the welding rod is increased and the hydrogen content of the weld is reduced, thereby improving the density of the weld. The fluorite content is then controlled to improve the weld formation and the fluidity of the slag. The rutile content is then controlled to improve the slag removal and weld formation of the welding rod. The micro-carbon ferrochromium content is then controlled to allow ferrite to be formed in the weld and chromium to be transferred into the weld, thereby ensuring that the corrosion resistance of the weld meets expectations. The molybdenum iron content is then controlled to promote the formation of ferrite. The niobium iron content is then controlled to introduce a small amount of niobium, thereby ensuring that the corrosion resistance of the weld meets expectations. The soda ash content is then controlled to improve the corrosion resistance of the weld in the deposition stage. Ensure that slag is sufficient and that the flux is an alkaline slag system. Then control the content of sodium alginate, increase the viscosity of the flux, and make sure that all raw materials are fully bonded. Finally, add rare earth elements and aluminum-zirconium alloys to the flux. Deoxidize the aluminum-zirconium alloy and refine the grains at the same time. Then use the rare earth elements to prevent the grains of the weld from being too large. At the same time, the rare earth elements can also reduce non-metallic impurities, making the weld structure pure and dense. Through the interaction between the rare earth elements and the aluminum-zirconium alloy, the effect of refining the grains is enhanced, which can not only make up for the lack of solid solution strength, but also improve the room temperature impact work in the welded and heat-treated states. Therefore, through the designed flux composition, the high-strength and high-toughness welding requirements required for the internal components of the nuclear power plant can be comprehensively obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0053] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0054] Figure 1 A schematic diagram of the metallographic structure of the heat-treated state at 400°C × 24h provided in the embodiment of the present application;

[0055] Figure 2 A schematic diagram of the metallographic structure of the 1050°C × 2h solution heat treatment state provided in the embodiment of the present application;

[0056] Figure 3 A schematic flow chart of a method for preparing a welding rod provided in an embodiment of the present application. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0058] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0059] The embodiment of the present application provides a coating of a welding rod for an internal component of a nuclear power plant. The raw materials of the coating include, by weight: marble: 19.0 to 23.0 parts, fluorite: 22.0 to 26.0 parts, rutile: 4.0 to 6.0 parts, wollastonite: 7.0 to 9.0 parts, micro-carbon ferrochrome: 13.5 to 16.5 parts, metallic nickel: 4.5 to 5.5 parts, electrolytic manganese: 2.5 to 3.5 parts, ferromolybdenum: 0.8 to 1.2 parts, ferroniobium: 0.2 to 0.4 parts, aluminum-zirconium alloy: 1.0 to 3.0 parts, rare earth: 2.0 to 3.0 parts, soda ash: 1.0 to 1.4 parts, and sodium alginate: 2.2 to 2.6 parts.

[0060] In the embodiment of the present application, the positive effect of the weight proportion of marble is 19.0 to 23.0 parts, and the positive effect is within the range of the weight proportion, because the main component of marble is CaCO 3 , decomposed under the action of welding arc heat to form CaO and CO 2Therefore, marble is a commonly used slag-making and gas-making material in the preparation of welding rods. It can increase the basicity of slag, refine molten droplets, stabilize arc, and has good desulfurization ability; at the same time, CO decomposed by marble 2 It reacts with manganese, silicon and titanium in the welding core or other coating materials to form oxides, which reduces the gas phase oxidizability, removes oxygen as early as possible, reduces the oxidation of the molten metal, and can directly react with hydrogen atoms in the arc atmosphere to remove hydrogen and reduce the hydrogen content of the weld.

[0061] The positive effect of the weight percentage of fluorite being 22.0 to 26.0 parts is that within this weight percentage range, since fluorite mainly contains CaF 2 During the welding process, slag with certain physical and chemical properties is formed, which plays a protective role and improves the weld formation. At the same time, it can also change the slag basicity, and CaF 2 It has a low melting point and can dilute the slag, thus improving its fluidity.

[0062] The positive effect of 4.0 to 6.0 parts by weight of rutile is within this weight range, because the main component of rutile is TiO 2 It can adjust the melting point of the slag, reduce the surface tension of the slag, ensure that the slag can evenly cover the upper surface of the weld, and improve the slag removal of the electrode and the weld formation.

[0063] The positive effect of wollastonite being 7.0 to 9.0 parts by weight is that within this weight range, wollastonite can increase the basicity of the welding material, adjust the viscosity and fluidity of the slag, facilitate the formation of short slag, and improve the welding process performance.

[0064] The positive effect of the weight proportion of micro-carbon ferrochrome being 13.5 to 16.5 parts is that within this weight proportion range, since micro-carbon ferrochrome is an alloying agent, it can transfer chromium elements to the weld, and is also the main element for forming ferrite, and is the main alloying element for stainless steel to obtain corrosion resistance.

[0065] The positive effect of the weight proportion of metallic nickel being 4.5 to 5.5 parts is that within this weight proportion range, since metallic nickel is an alloying agent, the use of powdered metallic nickel can transition the nickel element to the weld, thereby improving the performance of stainless steel in resisting corrosive media such as sulfuric acid and hydrochloric acid.

[0066] The positive effect of the electrolytic manganese content of 2.5 to 3.5 parts by weight is within this range of parts by weight, because electrolytic manganese is a good deoxidizer and desulfurizer; if the manganese content is very high, the oxidation resistance of the deposited metal will decrease.

[0067] The positive effect of the weight proportion of ferromolybdenum being 0.8 to 1.2 parts is that within this weight proportion range, since molybdenum is an element that forms ferrite, and adding molybdenum to the weld can improve the strength, corrosion resistance and stability of the weld in non-oxidizing media.

[0068] The positive effect of the 0.2 to 0.4 weight parts of ferroniobium is that within this weight range, the addition of a small amount of niobium can prevent the precipitation of chromium carbide at the grain boundaries of the steel, thereby improving the corrosion resistance of the steel.

[0069] The positive effect of the aluminum-zirconium alloy being 1.0 to 3.0 parts by weight is that within this weight range, since the aluminum-zirconium alloy is a strong deoxidizer, it also has the effect of refining the grains and improving the toughness of the weld, thereby compensating for the solid solution strengthening of the weld.

[0070] The positive effect of the rare earth content of 2.0 to 3.0 parts by weight is that within this weight range, the addition of rare earth can further refine the grains, purify weld impurities, and improve the weld plasticity and toughness.

[0071] The positive effect of soda ash being 1.0 to 1.4 parts by weight is within this range of parts by weight, because the main function of soda ash is to improve the coating properties of the electrode and increase the strength of the coating. At the same time, the sodium oxide generated by the decomposition of soda ash is an alkaline oxide and can be used as an important slag-forming agent.

[0072] The positive effect of the sodium alginate content of 2.2 to 2.6 parts by weight is that within this weight range, the presence of sodium alginate can increase the viscosity of the coating, thereby improving the electrode's pressure-coating property and eccentricity stability, so that the coating can be welded to the welding core to form a weld during the welding stage.

[0073] In some optional embodiments, based on the total weight of the marble, the particle size of the marble satisfies: 80 mesh ≥ 65 weight %; and / or,

[0074] Based on the total weight of the fluorite, the particle size of the fluorite satisfies: 50 mesh ≥ 96 weight %; and / or,

[0075] Based on the total weight of the rutile, the particle size of the rutile satisfies: 40 mesh ≥ 97 weight %; and / or,

[0076] Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 100 mesh ≥ 90 weight %; and / or,

[0077] Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome satisfies: 40 mesh ≥ 98 weight %; and / or,

[0078] Based on the total weight of the metallic nickel, the particle size of the metallic nickel satisfies: 60 mesh ≥ 95 weight %; and / or,

[0079] Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese satisfies: 40 mesh ≥ 98 weight %; and / or,

[0080] Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum satisfies: 40 mesh ≥ 98 weight %; and / or,

[0081] Based on the total weight of the ferroniobium, the particle size of the ferroniobium satisfies: 50 mesh ≥ 96 weight %; and / or,

[0082] Based on the total weight of the aluminum-zirconium alloy, the particle size of the aluminum-zirconium alloy satisfies: 60 mesh ≥ 97 weight %; and / or,

[0083] Based on the total weight of the rare earth, the particle size of the rare earth satisfies: 80 mesh ≥ 95 weight %; and / or,

[0084] Based on the total weight of the soda ash, the particle size of the soda ash satisfies: 80 mesh ≥ 98 weight %; and / or,

[0085] Based on the total weight of the sodium alginate, the particle size of the sodium alginate satisfies: 140 mesh ≥ 97 weight %.

[0086] In the embodiment of the present application, the particle size of each raw material of the electrode coating is controlled to ensure that the coating raw materials can be mixed evenly, so that the coating can be melted during the welding stage to form a weld with uniform composition, thereby improving the room temperature impact energy of the welded state and the heat-treated state, and obtaining welding requirements of high strength and high toughness required for the internal components of the nuclear power plant.

[0087] In some optional embodiments, based on the total weight of the marble, the particle size of the marble satisfies: 50 mesh ≥ 96 weight %; and / or,

[0088] Based on the total weight of the fluorite, the particle size of the fluorite is 30 mesh; and / or,

[0089] Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 50 mesh ≥ 97 weight %; and / or,

[0090] Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome is 30 mesh; and / or,

[0091] Based on the total weight of the metallic nickel, the particle size of the metallic nickel is 30 mesh; and / or,

[0092] Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese is 30 mesh; and / or,

[0093] Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum is 30 mesh.

[0094] In the embodiments of the present application, the particle size of the raw materials in the coating is further controlled to further ensure that the coating raw materials can be mixed evenly, so that the coating can be further melted during the welding stage to form a weld with uniform composition, thereby improving the room temperature impact energy in the welded and heat-treated states, and being able to obtain welding requirements of high strength and high toughness required for the internal components of the nuclear power plant.

[0095] In some optional embodiments, based on the total weight of the marble, the CaCO in the marble is 3 The content of ≥96% by weight; and / or,

[0096] Based on the total weight of the fluorite, the CaF 2 The content of ≥96% by weight; and / or,

[0097] Based on the total weight of the rutile, the TiO 2 The content of ≥95.5% by weight; and / or,

[0098] Based on the total weight of the wollastonite, the CaSiO 3 The content of ≥46.0% by weight; and / or,

[0099] Based on the total weight of the low-carbon ferrochrome, the content of Cr in the low-carbon ferrochrome is 65 wt% to 70 wt%; and / or,

[0100] Based on the total weight of the metallic nickel, the content of Ni in the metallic nickel is ≥ 99.5 wt %; and / or,

[0101] Based on the total weight of the electrolytic manganese, the content of Mn in the electrolytic manganese is ≥ 99.5 wt %; and / or,

[0102] Based on the total weight of the ferromolybdenum, the content of Mo in the ferromolybdenum is 55.0 wt% to 60.0 wt%, and the content of Fe in the ferromolybdenum is 40.0 wt% to 45.0 wt%; and / or,

[0103] Based on the total weight of the ferroniobium, the content of Nb in the ferroniobium is 50.0 wt% to 55.0 wt%, and the content of Fe in the ferroniobium is 45.0 wt% to 50.0 wt%; and / or,

[0104] Based on the total weight of the aluminum-zirconium alloy, the content of Al in the aluminum-zirconium alloy is 45.0 wt% to 50.0 wt%, and the content of Zr in the aluminum-zirconium alloy is 49.0 wt% to 51.0 wt%; and / or,

[0105] Based on the total weight of the rare earth, the content of rare earth elements in the rare earth is ≥ 83.0 wt %; and / or,

[0106] Based on the total weight of the soda ash, the Na 2 CO 3 The content of ≥98.5% by weight; and / or,

[0107] Based on the total weight of the sodium alginate, the Na 2 The content of O is 9.5 wt% to 13.0 wt%.

[0108] In the embodiments of the present application, the content of effective ingredients of each raw material in the coating is controlled to ensure the effect of each raw material in the coating, thereby improving the room temperature impact energy in the welded state and the heat-treated state, and obtaining welding requirements of high strength and high toughness that are required for the internal components of the nuclear power plant.

[0109] Based on a general inventive concept, the present application also provides a welding rod for a nuclear power plant internal component, the welding rod comprising the coating and a welding core, the coating coating being coated on the surface of the welding core.

[0110] The welding rod is realized based on the above-mentioned coating. The specific composition and content of the coating can refer to the above-mentioned embodiments. Since the welding rod adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0111] In some optional embodiments, the chemical composition of the welding core includes, by mass fraction: C≤0.007%, Mn: 1.5%~2.0%, Si≤0.20%, Cr: 21.5%~22.5%, Ni: 11.5%~12.5%, Mo≤0.1%, Cu≤0.05%, N≤0.025%, S≤0.005%, P≤0.010%, Co≤0.010%, V≤0.050%, and the balance is Fe and unavoidable impurities.

[0112] In the embodiments of the present application, the specific chemical composition of the welding core is controlled to ensure that the welding core is an ultra-low carbon chromium-nickel alloy stainless steel wire, thereby ensuring that the weld forms a system with low S content, low P content, and low impurity elements, thereby improving the room temperature impact energy in the welded and heat-treated states, and being able to obtain welding requirements of high strength and high toughness required for the internal components of the nuclear power plant.

[0113] The positive effect of C≤0.007% is that within this mass fraction range, the C content of the weld metal can be guaranteed to be less than 0.03%, so that the weld metal remains in an ultra-low carbon state and the corrosion resistance and crack resistance are improved.

[0114] The positive effect of the Mn mass fraction of 1.5% to 2.0% is that within this mass fraction range, it can achieve the transition of Mn elements between the welding core and the flux together with the electrolytic manganese in the flux, and reverse the burnout and stable transition of alloy elements during welding.

[0115] The positive effect of Si≤0.20% is that within this mass fraction range, the weld metal can be controlled to have a relatively low Si content, thereby improving the crack resistance of the weld metal.

[0116] The positive effect of the Cr mass fraction of 21.5% to 22.5% is that within this mass fraction range, the Cr element can be jointly transitioned between the welding core and the flux coating together with the micro-carbon ferrochrome in the flux coating, and the burn-in and stable transition of the alloy elements during the reverse welding process can be achieved. In combination with nickel elements, the oxidation resistance and thermal strength of the steel can be improved, and the corrosion resistance of the weld can be further improved.

[0117] The positive effect of Ni's mass fraction of 11.5% to 12.5% ​​is that within this mass fraction range, the Ni element can be jointly transferred between the welding core and the flux coating together with the metal nickel powder in the flux coating, thereby reversely compensating for the burnout and stable transfer of alloy elements during welding, and improving the performance of stainless steel after welding in resistance to corrosive media such as sulfuric acid and hydrochloric acid.

[0118] The positive effect of Mo≤0.1% is to control the molybdenum content within the expected range. At the same time, high molybdenum content will promote intermetallic phases in austenitic stainless steel, which will have an adverse effect on the corrosion resistance and mechanical properties of the steel, especially leading to a decrease in plasticity and toughness.

[0119] The positive effect of Cu≤0.05%, N≤0.025%, S≤0.005%, P≤0.010%, Co≤0.010%, and V≤0.050% is to ensure that the weld forms a system of low S content, low P content, and low impurity elements, thereby purifying the weld.

[0120] In some optional embodiments, the coating and the welding core are bonded by an adhesive, and the adhesive comprises a mixture of at least two water glass solutions.

[0121] In the embodiment of the present application, controlling the specific classification of the binder can ensure that the coating adheres to the surface of the welding core, while ensuring the strength of the coating and ensuring that the welding rod does not have eccentricity and coating cracking.

[0122] The mixed solution of water glass solution refers to a mixed solution of potassium-sodium water glass, wherein the mixed solution of potassium-sodium water glass includes a mixed solution of potassium-sodium water glass with a volume fraction of 75%, a modulus of 3.1, and a concentration of 42°Be' and a mixed solution of potassium-sodium water glass with a volume fraction of 25%, a modulus of 2.4, and a concentration of 46°Be'.

[0123] like Figure 3 As shown, based on a general inventive concept, the present application provides a method for preparing the welding rod, the method comprising:

[0124] S1. Mixing the raw materials of the drug coating of the first aspect to obtain a drug coating powder;

[0125] S2. Adding a binder to the coating powder to obtain a mixed powder;

[0126] S3. Wrapping the mixed powder on the surface of the welding core and baking it step by step to obtain a welding rod.

[0127] In the embodiment of the present application, the step-by-step baking method can prevent the coating of the welding rod from sticking and bubbling, thereby improving the drying quality.

[0128] The method is implemented for the above-mentioned welding rod, and the specific chemical composition of the welding rod can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be described one by one here.

[0129] In some optional embodiments, the mass ratio of the binder to the coating powder is 18% to 19%.

[0130] In the embodiment of the present application, the positive effect of controlling the mass ratio of the binder to the coating powder to be 18% to 19% is that within the range of the mass ratio, the binder and the coating powder can be ensured to be fully mixed, thereby ensuring sufficient bonding and wrapping between the coating powder and the welding core, thereby ensuring uniform distribution of components of subsequent welds, thereby improving the room temperature impact energy of the welded state and the heat-treated state, and being able to obtain welding requirements of high strength and high toughness required for the internal components of the nuclear power plant.

[0131] In some optional embodiments, the step-by-step baking includes a first baking stage and a second baking stage; the temperature of the first baking stage is 80° C. to 90° C., and the time of the first baking stage is 3.5 h to 4 h; and / or,

[0132] The temperature of the second baking stage is 370° C. to 380° C., and the time of the second baking stage is 2.5 h to 3 h.

[0133] In the embodiment of the present application, the positive effect of controlling the temperature of the first baking stage to 80°C to 90°C is that within this temperature range, the press-coated welding core can be first baked at a low temperature, thereby preventing the welding rod from sticking and bubbling and improving the drying quality.

[0134] The positive effect of controlling the time of the first baking stage to 3.5h to 4h is that within this time range, the press-coated welding core can be fully baked at low temperature, thereby preventing the welding rod from sticking and bubbling and improving the drying quality.

[0135] The positive effect of controlling the temperature of the second baking stage to 370°C to 380°C is that within this temperature range, the moisture of the drug coating can be discharged after high-temperature baking, thereby ensuring that the drug coating is dry and adheres without cracking.

[0136] The positive effect of controlling the time of the second baking stage to 2.5h to 3h is that within this time range, the drug coating can be sufficiently baked at a high temperature, so that the moisture in the drug coating is fully discharged, thereby ensuring that the drug coating is dry and adheres without cracking.

[0137] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0138] Example 1

[0139] A coating of a welding rod for a nuclear power plant internal component, wherein the raw materials of the coating include, by weight, 19.0 parts of marble, 26.0 parts of fluorite, 4.0 parts of rutile, 9.0 parts of wollastonite, 13.5 parts of micro-carbon ferrochrome, 5.5 parts of metallic nickel, 3.5 parts of electrolytic manganese, 0.8 parts of ferromolybdenum, 0.2 parts of ferroniobium, 3.0 parts of aluminum-zirconium alloy, 2.0 parts of rare earth, 1.0 parts of soda ash, and 2.6 parts of sodium alginate.

[0140] The chemical composition of the welding core of the welding rod includes, by mass fraction, C: 0.005%, Mn: 1.63%, Si: 0.16%, Cr: 21.80%, Ni: 11.30%, Mo: 0.0048%, Cu: 0.0054%, N: 0.012%, S: 0.0024%, P: 0.0063%, Co: 0.0027%, V: 0.0074%, and the balance is Fe and unavoidable impurities;

[0141] like Figure 2 As shown, a method for preparing a welding rod for a nuclear power plant internal component comprises:

[0142] S1. Mixing the raw materials of the drug coating of the first aspect to obtain a drug coating powder;

[0143] S2. Adding a binder to the coating powder to obtain a mixed powder;

[0144] S3. Wrap the mixed powder on the surface of the welding core through a welding rod hydraulic press, and bake it step by step to obtain a welding rod.

[0145] The mass ratio of the binder to the coating powder is 18.5%.

[0146] The step baking includes a first baking section and a second baking section; the temperature of the first baking section is 80°C, and the time of the first baking section is 4 hours; the temperature of the second baking section is 370°C, and the time of the second baking section is 3 hours.

[0147] Example 2

[0148] Comparing Example 2 with Example 1, the difference between Example 2 and Example 1 is:

[0149] The raw materials of the coating include: marble: 21.0 parts, fluorite: 24.0 parts, rutile: 5.0 parts, wollastonite: 8.0 parts, micro-carbon ferrochrome: 15 parts, metallic nickel: 5.0 parts, electrolytic manganese: 3.0 parts, ferromolybdenum: 1.0 parts, ferroniobium: 0.3 parts, aluminum-zirconium alloy: 2.0 parts, rare earth: 2.5 parts, soda ash: 1.2 parts, sodium alginate: 2.4 parts.

[0150] The step baking includes a first baking section and a second baking section; the temperature of the first baking section is 85°C, and the time of the first baking section is 3.5 hours; the temperature of the second baking section is 375°C, and the time of the second baking section is 2.5 hours.

[0151] Example 3

[0152] Comparing Example 3 with Example 1, the difference between Example 3 and Example 1 is:

[0153] The raw materials of the coating include: marble: 23.0 parts, fluorite: 22.0 parts, rutile: 6.0 parts, wollastonite: 7.0 parts, micro-carbon ferrochrome: 16.5 parts, metallic nickel: 4.5 parts, electrolytic manganese: 2.5 parts, ferromolybdenum: 1.2 parts, ferroniobium: 0.4 parts, aluminum-zirconium alloy: 1.0 parts, rare earth: 3.0 parts, soda ash: 1.4 parts, sodium alginate: 2.2 parts.

[0154] The step baking includes a first baking section and a second baking section; the temperature of the first baking section is 90°C, and the time of the first baking section is 3.5 hours; the temperature of the second baking section is 380°C, and the time of the second baking section is 2.5 hours.

[0155] Comparative Example 1

[0156] Comparative Example 1 and Example 1 are compared. The difference between Comparative Example 1 and Example 1 is:

[0157] The raw materials of the coating include: marble: 18.0 parts, fluorite: 27.0 parts, rutile: 3.0 parts, wollastonite: 10.0 parts, micro-carbon ferrochrome: 12.0 parts, metallic nickel: 6.5 parts, electrolytic manganese: 2.0 parts, ferromolybdenum: 2.0 parts, ferroniobium: 0.0 parts, aluminum-zirconium alloy: 0.0 parts, rare earth: 0.0 parts, soda ash: 1.0 parts, sodium alginate: 2.6 parts.

[0158] Comparative Example 2

[0159] Comparative Example 2 and Example 1 are compared. The difference between Comparative Example 2 and Example 1 is:

[0160] The raw materials of the coating include: marble: 24.0 parts, fluorite: 20.0 parts, rutile: 7.0 parts, wollastonite: 6.0 parts, micro-carbon ferrochrome: 18.0 parts, metallic nickel: 3.5.0 parts, electrolytic manganese: 4.0 parts, ferromolybdenum: 0.0 parts, ferroniobium: 0.6 parts, aluminum-zirconium alloy: 0.0 parts, rare earth: 0.0 parts, soda ash: 1.0 parts, sodium alginate: 2.6 parts.

[0161] Related experiments and effect data:

[0162] Welding experiments were conducted using the welding rods obtained in the embodiments and comparative examples, and the chemical composition and mechanical properties of the high-strength and high-toughness stainless steel welding rod deposited metal formed on the internal components of the nuclear power plant were measured. The results are shown in Tables 1 to 3.

[0163] Table 1 Chemical composition of deposited metal (%)

[0164]

[0165] Table 2 Mechanical properties of deposited metal

[0166]

[0167]

[0168] Table 3 Cold bending performance and corrosion resistance of deposited metal

[0169]

[0170] Detailed analysis of Tables 1 to 3:

[0171] It can be seen from the data of Examples 1-3 that by controlling the contents of marble, fluorite, rutile, micro-carbon ferrochrome, ferromolybdenum, ferroniobium, soda ash, and sodium alginate in the coating, and finally introducing rare earth elements and aluminum-zirconium alloys, and utilizing the interaction between the rare earth elements and the aluminum-zirconium alloys, the high-strength and high-toughness welding requirements for the internal components of the nuclear power plant can be comprehensively obtained through the designed coating composition.

[0172] And if Figure 1 and Figure 2 As shown, the weld formed by the welding rod obtained in Example 1 during the welding stage has high strength and high toughness in the heat treated state and the solution heat treated state, especially when the strength of the 400℃×24h dimensionally stabilized heat treated state is greater than 550MPa, and the room temperature impact resistance reaches more than 100J.

[0173] From the data of the embodiment and comparative examples 1 and 2, it can be seen that although the solid solution properties of comparative examples 1 and 2 can meet the requirements, the room temperature impact energy of the 400°C×24h dimensionally stabilized heat treated state is relatively low and cannot meet the requirements for the use of nuclear power plant internal components.

[0174] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0175] (1) The embodiment of the present application provides a coating of a welding rod for a nuclear power plant internal component. By controlling the contents of marble, fluorite, rutile, micro-carbon ferrochrome, ferromolybdenum, ferroniobium, soda ash, and sodium alginate in the coating, rare earth elements and aluminum-zirconium alloy are finally introduced. By utilizing the interaction between the rare earth elements and the aluminum-zirconium alloy, the coating composition is designed to comprehensively obtain the high-strength and high-toughness welding requirements for the nuclear power plant internal components.

[0176] (2) The embodiment of the present application provides a coating of a welding rod for a nuclear power plant internal component. By designing the coating composition and microalloying alloy system of the welding rod, the coating is generally an alkaline slag system during welding, thereby further improving the crack resistance and impact toughness of the weld.

[0177] (3) The embodiment of the present application provides a coating of a welding rod for the internal components of a nuclear power plant, which introduces rare earth elements and aluminum-zirconium alloy. The rare earth elements can prevent the coarsening of grains, improve the plasticity, toughness, oxidation resistance and corrosion resistance of the weld, improve the fluidity of the weld, reduce non-metallic impurities, and make the weld structure pure and dense, while the aluminum-zirconium alloy also has the function of deoxidation and grain refinement. By adopting fine grain strengthening, the impact toughness of the dimensionally stabilized heat-treated state can be improved, and the deficiency of reduced solid solution strength can be compensated.

[0178] (4) The embodiment of the present application provides a welding rod for the internal components of a nuclear power plant, which uses a refined ultra-low carbon chromium-nickel alloy stainless steel wire as a welding core, and determines a system of low S, low P, and low impurity elements in the weld.

[0179] (5) The embodiment of the present application provides a welding rod for the internal components of a nuclear power plant. During the welding process, the arc is stable, the spatter is small, and the slag removal performance is good. The welding can be performed in all positions, including flat welding, horizontal welding, vertical welding, and overhead welding. The weld metal can simultaneously meet the requirements of high strength and high toughness in both the dimensionally stabilized heat treated state and the solution heat treated state. The weld metal has excellent mechanical properties, especially the strength in the dimensionally stabilized heat treated state is greater than 550MPa, the room temperature impact resistance reaches more than 100J, and the weld metal also has excellent corrosion resistance.

[0180] Explanation of the attached figure:

[0181] Figure 1 A schematic diagram of the metallographic structure of the heat-treated state at 400°C × 24h provided in the embodiment of the present application;

[0182] Figure 2 A schematic diagram of the metallographic structure of the 1050°C × 2h solution heat treatment state provided in the embodiment of the present application;

[0183] Depend on Figure 1 It can be seen that the metallographic structure of the present application is evenly distributed and has fine grains, which indicates that the impact toughness of the dimensionally stabilized heat-treated state of the present application is high and the strength of the solution heat-treated state is high.

[0184] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0185] In this application, unless otherwise specified, directional words such as "upper" and "lower" used refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of this application, the terms "include", "comprise", etc. mean "including but not limited to".

[0186] In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, c can be single or multiple respectively.

[0187] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A welding rod for a nuclear power plant internal component, characterized in that: The welding rod comprises a coating and a welding core, wherein the coating is coated on the surface of the welding core, and the raw materials of the coating are composed of 19.0 to 23.0 parts of marble, 22.0 to 26.0 parts of fluorite, 4.0 to 6.0 parts of rutile, 7.0 to 9.0 parts of wollastonite, 13.5 to 16.5 parts of micro-carbon ferrochrome, 4.5 to 5.5 parts of metallic nickel, 2.5 to 3.5 parts of electrolytic manganese, 0.8 to 1.2 parts of ferromolybdenum, 0.2 to 0.4 parts of ferroniobium, 1.0 to 3.0 parts of aluminum-zirconium alloy, 2.0 to 3.0 parts of rare earth, 1.0 to 1.4 parts of soda ash, and 2.2 to 2.6 parts of sodium alginate; The chemical composition of the welding core includes, by mass fraction, C≤0.007%, Mn: 1.5%-2.0%, Si≤0.20%, Cr: 21.5%-22.5%, Ni: 11.5%-12.5%, Mo≤0.1%, Cu≤0.05%, N≤0.025%, S≤0.005%, P≤0.010%, Co≤0.010%, V≤0.050%, and the balance is Fe and unavoidable impurities; The coating and the welding core are bonded by an adhesive, wherein the adhesive comprises a mixture of at least two water glass solutions, wherein the mixture of the two water glass solutions is a mixture of potassium-sodium water glass with a volume fraction of 75%, a modulus of 3.1, and a concentration of 42°Be', and a mixture of potassium-sodium water glass with a volume fraction of 25%, a modulus of 2.4, and a concentration of 46°Be'.

2. The welding rod according to claim 1, characterized in that Based on the total weight of the marble, the particle size of the marble satisfies: 80 mesh ≥ 65 weight %; and / or, Based on the total weight of the fluorite, the particle size of the fluorite satisfies: 50 mesh ≥ 96 weight %; and / or, Based on the total weight of the rutile, the particle size of the rutile satisfies: 40 mesh ≥ 97 weight %; and / or, Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 100 mesh ≥ 90 weight %; and / or, Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome satisfies: 40 mesh ≥ 98 weight %; and / or, Based on the total weight of the metallic nickel, the particle size of the metallic nickel satisfies: 60 mesh ≥ 95 weight %; and / or, Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese satisfies: 40 mesh ≥ 98 weight %; and / or, Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum satisfies: 40 mesh ≥ 98 weight %; and / or, Based on the total weight of the ferroniobium, the particle size of the ferroniobium satisfies: 50 mesh ≥ 96 weight %; and / or, Based on the total weight of the aluminum-zirconium alloy, the particle size of the aluminum-zirconium alloy satisfies: 60 mesh ≥ 97 weight %; and / or, Based on the total weight of the rare earth, the particle size of the rare earth satisfies: 80 mesh ≥ 95 weight %; and / or, Based on the total weight of the soda ash, the particle size of the soda ash satisfies: 80 mesh ≥ 98 weight %; and / or, Based on the total weight of the sodium alginate, the particle size of the sodium alginate satisfies: 140 mesh ≥ 97 weight %.

3. The welding rod according to claim 2, characterized in that Based on the total weight of the marble, the particle size of the marble satisfies: 50 mesh ≥ 96 weight %; and / or, Based on the total weight of the fluorite, the particle size of the fluorite is 30 mesh; and / or, Based on the total weight of the wollastonite, the particle size of the wollastonite satisfies: 50 mesh ≥ 97 weight %; and / or, Based on the total weight of the micro-carbon ferrochrome, the particle size of the micro-carbon ferrochrome is 30 mesh; and / or, Based on the total weight of the metallic nickel, the particle size of the metallic nickel is 30 mesh; and / or, Based on the total weight of the electrolytic manganese, the particle size of the electrolytic manganese is 30 mesh; and / or, Based on the total weight of the ferromolybdenum, the particle size of the ferromolybdenum is 30 mesh.

4. The welding rod according to claim 1, characterized in that The content of CaCO3 in the marble is ≥ 96 wt% based on the total weight of the marble; and / or, Based on the total weight of the fluorite, the content of CaF2 in the fluorite is ≥ 96 wt%; and / or, Based on the total weight of the rutile, the content of TiO2 in the rutile is ≥ 95.5 wt%; and / or, Based on the total weight of the wollastonite, the content of CaSiO3 in the wollastonite is ≥46.0 wt%; and / or, Based on the total weight of the low-carbon ferrochrome, the content of Cr in the low-carbon ferrochrome is 65 wt% to 70 wt%; and / or, Based on the total weight of the metallic nickel, the content of Ni in the metallic nickel is ≥ 99.5 wt %; and / or, Based on the total weight of the electrolytic manganese, the content of Mn in the electrolytic manganese is ≥ 99.5 wt %; and / or, Based on the total weight of the ferromolybdenum, the content of Mo in the ferromolybdenum is 55.0 wt% to 60.0 wt%, and the content of Fe in the ferromolybdenum is 40.0 wt% to 45.0 wt%; and / or, Based on the total weight of the ferroniobium, the content of Nb in the ferroniobium is 50.0 wt% to 55.0 wt%, and the content of Fe in the ferroniobium is 45.0 wt% to 50.0 wt%; and / or, Based on the total weight of the aluminum-zirconium alloy, the content of Al in the aluminum-zirconium alloy is 45.0 wt% to 50.0 wt%, and the content of Zr in the aluminum-zirconium alloy is 49.0 wt% to 51.0 wt%; and / or, Based on the total weight of the rare earth, the content of rare earth elements in the rare earth is ≥ 83.0 wt %; and / or, The content of Na2CO3 in the soda ash is ≥ 98.5 wt% based on the total weight of the soda ash; and / or, Based on the total weight of the sodium alginate, the content of Na2O in the sodium alginate is 9.5 wt% to 13.0 wt%.

5. A method for preparing the welding rod according to any one of claims 1 to 4, characterized in that: The method comprises: Mixing raw materials for the medicine coating to obtain medicine coating powder; Adding a binder to the coating powder to obtain a mixed powder; The mixed powder is coated on the surface of the welding core and baked step by step to obtain a welding rod.

6. The method according to claim 5, characterized in that The mass ratio of the binder to the coating powder is 18% to 19%.

7. The method according to claim 5, characterized in that The stepwise baking comprises a first baking stage and a second baking stage; the temperature of the first baking stage is 80° C. to 90° C., and the time of the first baking stage is 3.5 h to 4 h; and / or, The temperature of the second baking stage is 370° C. to 380° C., and the time of the second baking stage is 2.5 h to 3 h.