A method and device for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid

Through the premix of artificial rutile waste liquid with calcium carbonate suspension and sodium hydroxide reaction, combined with the participation of ammonium dihydrogen phosphate and hydrogen peroxide, the efficient production of battery-grade iron phosphate is achieved, solving the problems of low resource utilization and environmental pollution. Meets the new energy industry's demand for high-quality raw materials.

CN115924870BActive Publication Date: 2024-10-15SHANDONG LUBEI ENTERPRISE GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211577295.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-15
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

When processing artificial rutile waste liquid, the resource utilization rate is low, the production efficiency and product purity are insufficient, and the environmental pollution pressure is high, making it difficult to meet the new energy industry's demand for high-quality and low-cost raw materials.

Method used

By premixing the artificial rutile waste liquid with calcium carbonate suspension, the pH value is controlled to be 2-3, and then reacting with sodium hydroxide solution. After filtration, ammonium dihydrogen phosphate and hydrogen peroxide are added to synthesise iron phosphate. The series connection and connection of grade equipment and circulation structures can achieve high-quality continuous production of battery-grade iron phosphate.

Benefits of technology

It has achieved high-quality and low-cost battery-grade iron phosphate production, improved resource utilization, reduced sewage treatment costs, and reduced environmental pollution, meeting the demand for high-quality raw materials in the new energy industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115924870B_ABST
    Figure CN115924870B_ABST
Patent Text Reader

Abstract

The present invention relates to a method and device for preparing iron phosphate and co-producing white gypsum by utilizing artificial rutile waste liquid. The method and device can realize the effective and high-quality continuous production of battery-grade iron phosphate products, and provide an effective, high-quality and low-cost source of raw materials for iron batteries, such as lithium iron phosphate, which are currently of widespread concern in the new energy industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a preparation process and equipment for a chemical product, and specifically to a method and device for co-producing white gypsum with iron phosphate produced through waste acid liquid, and in particular to a method and device for co-producing white gypsum with battery-grade iron phosphate that can be used for power battery production. Background Art

[0002] At present, the treatment of artificial rutile waste liquid at home and abroad is to produce ferrous sulfate heptahydrate and polyferric sulfate as a water purifier through a ferrous crystallization system, and the acidic wastewater after crystallization is sent to sewage treatment. The production process of artificial rutile will produce a large amount of iron-containing acidic wastewater. If it is directly sent to sewage treatment, the resources cannot be fully utilized. At the same time, the treatment of wastewater will increase the company's operating costs. The comprehensive utilization of artificial rutile waste liquid can not only bring economic benefits to the company, but also reduce the cost of sewage treatment. Therefore, how to use a large amount of waste acid and make full use of resources has become the key to the development of the company.

[0003] However, even with the existing technology for treating waste acid liquid, the product added value of ferrous sulfate and polyferric sulfate water purifiers is low, the market prospects are not broad enough, and the pressure on the environment has not been significantly reduced. From the perspective of sustainable development, it is not the most ideal choice.

[0004] On the contrary, the new energy industry, especially the new energy industry related to lithium batteries (such as automobiles and energy storage) is the country's emerging industry and future development direction. If the large amount of artificial rutile waste liquid can be linked to the new energy lithium battery industry, it will be an effective development direction for future industrial technology.

[0005] However, in the process of manufacturing lithium battery raw materials from artificial rutile waste liquid, there are still many obstacles to industrial large-scale production, such as production efficiency, environmental pollution, purity and quality of products.

[0006] Therefore, there is a need in the art to solve one or more of the above-mentioned technical problems. Summary of the invention

[0007] Based on the above related technologies, one aspect of the present invention provides a method for preparing (battery-grade) iron phosphate and co-producing white gypsum using artificial rutile waste liquid. The method can achieve effective and high-quality continuous production of battery-grade iron phosphate products, and provide an effective, high-quality, and low-cost source of raw materials for iron batteries (such as lithium iron phosphate) that are currently of widespread concern in the new energy industry.

[0008] Another aspect of the present invention provides a device for preparing (battery-grade) iron phosphate and co-producing white gypsum using artificial rutile waste liquid, which helps to achieve the preparation of battery-grade iron phosphate through the series connection and connection of multi-stage equipment and circulation structures.

[0009] In a first aspect of the present invention, a method for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid is provided, the method comprising the following steps:

[0010] Step a): artificial rutile waste liquid and calcium carbonate suspension are pumped into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows into a neutralization tank for further neutralization reaction. During the reaction, the pH of the system is controlled to be 2-3, and after the reaction, a ferrous sulfate solution with a pH of about 2 to 3 is obtained through a gypsum filter press;

[0011] Step b): adding the ferrous sulfate solution obtained in step a) to a ferrous sulfate purification reaction tank by a metering pump, adding a sodium hydroxide solution to keep the pH value of the solution at about 4 to 6, preferably adjusted to about 4 to 5, more preferably adjusted to 4 to 4.5, and heating to 70-80° C. for heat preservation; thereafter, the reaction solution is placed in a sedimentation tank, filtered through a microporous filter to obtain a purified ferrous sulfate solution and slurry, and the ferrous sulfate solution is sent to a ferrous sulfate metering tank via a ferrous sulfate storage tank;

[0012] Step c): adding ammonia water and diammonium phosphate solid (preferably, the mother liquor filtered through a microporous filter after the reaction cycle is completed) into a diammonium phosphate dissolving tank to dissolve the diammonium phosphate to obtain a diammonium phosphate solution;

[0013] Step d): adding the ferrous sulfate solution in step a) into the ferric phosphate synthesis kettle, mixing the ammonium dihydrogen phosphate solution and the hydrogen peroxide solution uniformly, first pumping them into the ammonium salt metering tank, and then dripping them into the ferric phosphate synthesis kettle for reaction;

[0014] Step e): the iron phosphate obtained after the reaction in step d) is pumped into a first filter press for filtration and washing, the washed iron phosphate is slurried and pumped into an aging kettle, phosphoric acid is added into the aging kettle, and the aging is carried out for 30-90 minutes by heating; the obtained iron phosphate is further sent to a second filter press for filtration and washing to obtain an iron phosphate filter cake;

[0015] Step f): The iron phosphate filter cake obtained in step e) is sent to a dryer (such as a flash dryer) for dehydration, then calcined in a calcining kiln (such as a rotary kiln), and then crushed in a steam pulverizer to obtain battery-grade iron phosphate.

[0016] In an optional scheme, the method further includes: step g): wastewater recycling and reuse: adding ammonia water to the first wash filtrate and washing water obtained in the step e) to adjust the pH value, then removing trace impurities through an inclined plate sedimentation tank and a filtering device, the filtrate is passed through a reverse osmosis device to produce desalted water, and the desalted water is concentrated into a liquid to prepare ammonium sulfate; and the second wash filtrate obtained in the step e) is passed through a microporous filter to obtain a mother liquor, the mother liquor is returned for the preparation of diammonium phosphate, and the washing water of the second wash step is further returned to the first wash filter press as washing water for the first wash.

[0017] In an optional embodiment, the method is carried out by the following steps:

[0018] Step a): converting the actual sulfuric acid content to the actual calcium carbonate content, and pumping the artificial rutile waste liquid with a sulfuric acid content of 8wt% to 15wt% and the calcium carbonate suspension with a calcium carbonate content of 200-400g / L into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows to a neutralization tank for further neutralization reaction, and the neutralization reaction time is 1-3 hours. After the reaction, a ferrous sulfate solution with a pH of 2 to 3 is obtained through a gypsum filter press;

[0019] Step b): adding the ferrous sulfate solution of step a) into a ferrous purification reaction tank by a metering pump, adding a sodium hydroxide solution with a mass content of about 10wt% to 20wt%, preferably adjusting the pH value of the solution to 4 to 5, more preferably to 4 to 4.5, heating to 60-85°C, keeping warm for 0.5 to 2 hours, placing in a sedimentation tank, and filtering through a microporous filter when the temperature drops below 60 degrees Celsius to obtain a purified ferrous sulfate solution and mud, the ferrous sulfate solution is sent to the next step, and the mud is sent to a sewage treatment station for treatment;

[0020] Step c): adding ammonia water and diammonium phosphate solid (preferably, the mother liquor filtered through a microporous filter after the reaction cycle is completed) with a mass concentration of 10-30wt% to a diammonium phosphate dissolving tank at a molar ratio of the substances contained (1.0-1.1):1 to dissolve the diammonium phosphate to obtain a diammonium phosphate solution; filtering through an ammonium salt filter press to obtain a pure diammonium phosphate solution.

[0021] Step d): pump the ferrous sulfate solution into the ferrous sulfate metering tank, then add it into the ferric phosphate synthesis kettle, mix the diammonium hydrogen phosphate solution and the hydrogen peroxide solution with a mass concentration of about 20-25wt% evenly, then pump it into the metering tank, and drop it into the ferric phosphate synthesis kettle for 30-60 minutes, control the reaction temperature at 60°C, and continue the reaction for 1 hour after the dropwise addition.

[0022] Step e): The iron phosphate obtained by the reaction is pumped into a first-wash filter press for filtration and washing, and the washing is stopped when the conductivity of the washing water is ≤3500 microsiemens / cm. After the iron phosphate is slurried, it is pumped into an aging kettle, phosphoric acid is added, and it is heated to 70-90 degrees Celsius for aging for 60-120 minutes. The jacketed coil is cooled to below 55 degrees Celsius and enters a second-wash filter press for filtration and washing; the iron phosphate filter cake is sent to the next step via a belt conveyor.

[0023] Step f): The iron phosphate filter cake is first sent to a flash dryer via a screw conveyor to remove surface water, then calcined in a rotary kiln to remove crystal water, then crushed in a steam powder mill, and finally packaged to obtain battery-grade iron phosphate.

[0024] Step g): wastewater recycling and reuse: ammonia water is added to the first wash filtrate and washing water to adjust the pH in the regulating tank, and trace impurities such as organic matter are removed through the inclined plate sedimentation tank and the filtering equipment. The filtrate is passed through the reverse osmosis device to produce desalted water, and the desalted water is concentrated into liquid to produce ammonium sulfate; the second wash filtrate is passed through a microporous filter to obtain a mother liquor, which is returned for the preparation of diammonium phosphate, and the second wash water is returned to the first wash filter press as the washing water of the first wash.

[0025] In an optional solution, the pH value of the control system in step a) is achieved by spraying a sulfuric acid solution or a calcium hydroxide solution with a molar concentration not exceeding 0.1 mol / L into the neutralization tank.

[0026] In an optional scheme, the reaction in step a) is carried out by a neutralization tank, which comprises a tank body, an acid-base spray port extending from the bottom of the tank body into the tank body, and a pH monitor also extending from the bottom of the tank body into the tank body, wherein the acid-base spray port selects to spray sulfuric acid solution, water or calcium hydroxide solution according to feedback data from the pH monitor to maintain the pH of the reaction system at 2 to 3; and

[0027] The acid-base spray port is capable of rotating around its own axis and is arranged at the lower part of the trough body, more preferably, at 1 / 3 or lower of the entire height of the trough body from the bottom; the pH value monitor is preferably arranged at an upper position around the acid-base spray port, preferably at a position immediately above it.

[0028] Another aspect of the present invention provides a device for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid, characterized in that the device comprises a ferrous sulfate manufacturing and co-producing gypsum equipment, a phosphate supply equipment, an iron phosphate synthesis equipment and optional auxiliary equipment; wherein:

[0029] The ferrous sulfate manufacturing and gypsum co-production equipment comprises an artificial rutile waste acid storage tank, a calcium carbonate suspension storage tank, a premixing tank, a neutralization tank, a gypsum filter press, a ferrous purifying reaction tank, a settling tank, a microporous filter and a ferrous sulfate storage tank; and the outlets of the artificial rutile waste acid storage tank and the calcium carbonate suspension storage tank are connected to the inlet of the premixing tank; the outlet of the premixing tank is preferably directly connected to the inlet of the neutralization tank; the outlet of the neutralization tank, the gypsum filter press, the ferrous purifying reaction tank, the settling tank, the microporous filter and the ferrous sulfate storage tank are connected in sequence; and

[0030] The phosphate providing equipment comprises a diammonium phosphate dissolving tank, an ammonium salt filter press and a diammonium phosphate storage tank which are connected in sequence; preferably, the diammonium phosphate dissolving tank is also connected to an ammonia water and diammonium phosphate inlet, and is also equipped with a mother liquor receiving device for receiving mother liquor returned from the iron phosphate reaction after the preparation is completed;

[0031] The ferric phosphate synthesis equipment includes a ferric phosphate synthesis kettle, an ammonium salt metering tank, a ferrous iron metering tank and a hydrogen peroxide storage tank directly or indirectly connected to the ferric phosphate synthesis kettle. In addition, the outlet of the ferric phosphate synthesis kettle is sequentially connected to a wash filter press, a wash pulping tank, an aging kettle and a ferric phosphate storage tank.

[0032] In an optional scheme, the auxiliary equipment includes a secondary wash filter press, a microporous filter, and a thick slurry tank connected to the outlet of the iron phosphate storage tank and arranged in sequence, and the outlet of the thick slurry tank is connected to the primary wash filter press; and / or, a regulating tank connected to the waste liquid outlet of the primary wash filter press, and an inclined plate sedimentation tank, a filtration device, a reverse osmosis device, and an ammonium sulfate generating device connected to the regulating tank in sequence; it may also include an iron phosphate filter cake conveying device, a dryer, a rotary kiln, a steam powder machine, and a packaging machine connected to the secondary wash filter press.

[0033] In an optional solution, the neutralization tank includes a tank body, an acid-base spray port extending from the bottom of the tank body into the tank body, and a pH value monitor also extending from the bottom of the tank body into the tank body; and

[0034] The acid-base spray port can rotate around its own axis and is arranged at the lower part of the tank body, more preferably, at 1 / 3 or lower of the entire height of the tank body 1 from the bottom; the pH value monitor is preferably arranged at an upper position close to the acid-base spray port, preferably at a position immediately above it.

[0035] In an optional solution, the device is used to implement any one or more processes in the above-mentioned methods.

[0036] In the following, the technical solutions and advantages of the present invention will be explained and described in more detail in conjunction with specific implementation methods. It should be understood that the contents presented in the specification and specific implementation methods are only for the purpose of more clearly illustrating the technical solutions and advantages of the present invention, and do not limit the protection scope of the present invention. Those skilled in the art can obtain the changed technical solutions based on the disclosure of the specification for various reasonable transformations. As long as they do not deviate from the spirit of the present invention, the various changed technical solutions should be understood to be included in the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings are used to provide a further understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the specific embodiments of the present application, they are used to explain the technical solution of the present disclosure and do not constitute a limitation on the technical solution of the present disclosure.

[0038] Figure 1 is a flow chart of the preparation process and manufacturing equipment of the present invention;

[0039] Figure 2 It is the neutralization tank (which can also be used as a purification reaction tank) adopted by the present invention. DETAILED DESCRIPTION

[0040] The present invention is described in more detail hereinafter to facilitate understanding of the invention.

[0041] Before describing the specific implementation scheme, the sources of some of the main raw materials used are described in this specification. It should be noted that the sources of raw materials described in the specific implementation scheme here are non-restrictive. Those skilled in the art can select appropriate raw materials and test equipment to carry out relevant tests and obtain corresponding results based on the enlightenment and teaching of the present invention. For raw materials that do not specify specific manufacturers or pathways, those skilled in the art can select raw materials that meet corresponding requirements as reaction starting materials based on the disclosure content and requirements of this specification. The reaction raw materials for synthesizing some compounds come from the initial products synthesized in the preamble step of the present invention, which is also understandable based on the disclosure of the specification of the present invention.

[0042] The artificial rutile waste liquid used in the embodiment of the present invention comes from the waste acid liquid produced by reducing, roasting and acid leaching high-titanium slag (wherein the titanium dioxide content is more than 50wt%) produced from ilmenite in Tanzania and Australia in Africa to produce artificial rutile. The sulfuric acid content in the produced waste acid liquid is 8.5wt% to 10wt% of the entire waste liquid. The waste acid liquid is filtered and precipitated to remove slag. In addition to very few other impurities, it mainly contains titanium ions (mainly tetravalent titanium ions Ti) accounting for about 1.0wt% to 1.5wt% of the waste liquid. 4+ ) and containing 5.5wt% to 6wt% of ferrous ions (Fe2+ ).

[0043] Gypsum filter press: The filter press of the present application can be selected from commercially available filter press equipment. In a specific embodiment of the present invention, a plate-frame filter press provided by Shandong Zhucheng Boyu Environmental Protection Equipment Co., Ltd. is used. The filter cloth of the filter press is selected from Bolian Filtration Co., Ltd. The filter cloth provided for the plate and frame filter press has a mesh size of 200 mesh (mesh diameter is about 75 μm).

[0044] In the process and corresponding device for preparing the co-production of white gypsum of iron phosphate using artificial rutile waste liquid designed by the inventor, no matter which type of gypsum filter press is used, it is reasonable to select and determine the mesh size of the filter press filter cloth to promote the efficiency of the co-production process. In a suitable process, the mesh size of the filter press filter cloth is between about 150 meshes and 300 meshes, preferably selected from between 180 meshes and 250 meshes. When the mesh size is larger than the selected size (e.g., the mesh number is less than 180 meshes or less than 150 meshes), it is not conducive to the filtration and deviating of (white) gypsum after the reaction, and some gypsum products may enter the next process link through the mesh for unnecessary circulation and waste, and the impurities of subsequent ferrophosphorus materials may also rise. When the mesh size is smaller than the selected size (e.g., the mesh number is greater than 250 meshes or greater than 300 meshes), even if the filtration and chemical reaction process are optimized, it is not most conducive to the rapid filtration of gypsum filtrate, and it may also cause the filter cloth to be damaged or blocked to a certain extent.

[0045] Embodiment 1:

[0046] Step a, convert the artificial rutile waste liquid and the calcium carbonate suspension with a calcium carbonate content of 270g / L according to the actual sulfuric acid content and the actual calcium carbonate content, and according to the actual solute (substance) molar ratio of 1.5:1, pump them into the premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows to the neutralization tank for further neutralization reaction. The neutralization reaction time is 2h. After the reaction, a ferrous sulfate solution with a pH of 2-3 is obtained through a white gypsum filter press. This step requires that the pH value cannot be greater than 3, otherwise the titanium part in the solution will be hydrolyzed, which is easy to clog the filter cloth and make filter pressing difficult. Optionally, the (white) gypsum of the present application can be used as a raw material for the "gypsum-based sulfuric acid co-production cement device".

[0047] The inventors found in the process of preparing ferric phosphate of the present invention that in the acidic ferrous sulfate and Ti ion solution, when the pH value is slightly higher than the predetermined value, the titanium ion will hydrolyze to generate crystalline flocculent metatitanic acid (e.g., H2TiO3). The hydrolysis process of Ti ions is relatively complicated. In a non-restrictive manner, in the presence of reaction heat, when the pH value is not within the expected range, the reaction of TiOSO4+2H2O-H2TiO3+H2SO4 occurs. The undesirable hydrolysis of the Ti element / ion in this step is not only incorporated into the future white gypsum raw material to produce undesirable impurities, but more importantly, it causes the filter press to gradually become blocked in industrial production, and it is often necessary to stop the assembly line production to clean the filter press filter cloth, resulting in a reduction in production efficiency.

[0048] In the above step a), in order to obtain satisfactory raw materials and products that can be produced continuously and of high quality, it is preferred to use an improved neutralization tank device, which will be described in detail in Example 2.

[0049] Step b, adding the ferrous sulfate solution into the ferrous purification reaction tank by a metering pump, adding a sodium hydroxide solution with a mass content of about 16wt%, adjusting the solution pH to 4 to 6, preferably to 4 to 5, more preferably to 4 to 4.5, heating to 70-80°C, keeping warm for 1h, placing in a sedimentation tank, and filtering through a microporous filter when the temperature drops below 60 degrees Celsius to obtain a purified ferrous sulfate solution and mud, the ferrous sulfate solution is sent to the next step, and the mud is sent to a sewage treatment station for treatment.

[0050] In this step, the control of pH value will also have an impact on production efficiency and product purity. After step a) ends, Ti ions in the waste liquid will follow and enter the slurry. In step b), the control of pH value is implemented so that Ti ions are fully hydrolyzed, precipitated and separated in this step, so that they are removed in the aging tank and the non-porous filtration. In step b), when the pH value is adjusted to more than 3 by sodium hydroxide solution, some Ti ions will gradually hydrolyze, but until more than 4, the hydrolysis part will be carried out more fully. Here, the pH value is not preferably more than 6, and it is particularly not preferably more than 7. Ferrous ions are more sensitive to alkaline environments. When approaching or exceeding the acid-base balance, it is easy to generate Fe precipitates, resulting in reduced production efficiency. In the present application, since the process is suitable for large-scale continuous production, an alkaline solution with a large concentration is used, such as a sodium hydroxide solution with a content of about 16wt%. At this time, the difficulty of pH control increases, so it is preferred that the pH value does not exceed 6 to ensure that Fe ions will not precipitate or over-precipitate.

[0051] In the preferred embodiment of the present invention, the purification reaction tank can adopt the same neutralization tank equipment as step a). Sodium hydroxide and sulfuric acid solutions are arranged in the corresponding nozzles, and the pH value is controlled to be within the above range (4 to 6) in linkage with the nearby pH value detector.

[0052] Step c, adding ammonia water with a mass concentration of 25wt% and diammonium phosphate solid (preferably, the mother liquor filtered through a microporous filter after the reaction cycle is completed) in proportion to a diammonium phosphate dissolving tank, dissolving the diammonium phosphate to obtain a diammonium phosphate solution. After filtering through an ammonium salt filter press, a pure diammonium phosphate solution is obtained.

[0053] Step d, pump the ferrous sulfate solution into the ferrous sulfate metering tank, then add it into the ferric phosphate synthesis kettle, mix the ammonium dihydrogen phosphate solution and the hydrogen peroxide solution with a mass concentration of about 23wt% evenly, then pump it into the metering tank, and add it dropwise into the ferric phosphate synthesis kettle. It takes about 40 minutes, and the reaction temperature is controlled at 60°C. After the addition is completed, the reaction is continued for 1 hour.

[0054] Step e: pump the ferric phosphate into the first filter press for filtration and washing, stop washing when the conductivity of the washing water is ≤3500 microsiemens / cm, pump the ferric phosphate into the aging kettle after pulping, add phosphoric acid, heat to 90 degrees Celsius for aging for 90 minutes, cool the jacketed coil to below 55 degrees Celsius and enter the second filter press for filtration and washing. The ferric phosphate filter cake is sent to the next step via a belt conveyor.

[0055] Step f: The ferric phosphate filter cake is first conveyed to a dryer (such as a flash dryer) via a screw conveyor to remove surface water, then calcined in a calcining kiln (such as a rotary kiln) to remove crystal water, then crushed in a steam powder mill, and finally packaged and stored.

[0056] Optionally, the process of the present invention may further include a recycling device:

[0057] Step g, wastewater recycling and reuse: Ammonia water is added to the first wash filtrate and washing water to adjust the pH in the regulating tank, and trace impurities such as organic matter are removed through the inclined plate sedimentation tank and filtering equipment. The filtrate is passed through the reverse osmosis device to produce desalted water, and the desalted water is concentrated into liquid to produce ammonium sulfate; ammonium sulfate can be used as fertilizer. The second wash filtrate is passed through a microporous filter to obtain a mother liquor, which can be returned for the preparation of diammonium phosphate, and the second wash water can also be returned to the first wash filter press as the first wash water.

[0058] The process of Example 1 is as follows Figure 1 and Figure 2 The equipment room represented is executed. The equipment part will be described in detail below.

[0059] Figure 1 The process of the embodiment of the present invention can be exemplified.

[0060] exist Figure 1Solid iron phosphate product was extracted from test point 3 (iron phosphate filter cake) for testing, and the test results showed that the impurity contents of the iron phosphate product manufactured by the process of the present application were better than the chemical industry standard of the People's Republic of China "HG / T4701-2014 Iron Phosphate for Batteries".

[0061] Table 1: Test results of iron phosphate prepared in Example 1

[0062]

[0063]

[0064] Example 2

[0065] Device for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid. It should be noted that the device described below can execute the method of Example 1, or can modify or transform the method of Example 1. When there are no special components, subsystems, or devices described in this embodiment, those skilled in the art can assemble and connect them using commercially available or existing components according to the description of this specification. The technical solution of the present invention may include the various components shown in Example 2, or may only consist of the components / structures described in Example 2.

[0066] The device for preparing iron phosphate and co-producing gypsum using artificial rutile waste liquid includes ferrous sulfate co-producing gypsum equipment, phosphate supply equipment, iron phosphate synthesis equipment and optional auxiliary equipment. The description of the device of the present invention can be referred to Figure 1 and Figure 2 Description.

[0067] The ferrous sulfate manufacturing and co-production of gypsum equipment includes an artificial rutile waste acid storage tank, a calcium carbonate suspension storage tank, a premixing tank, a neutralization tank, a gypsum filter press, a ferrous sulfate purification reaction tank, a sedimentation tank, a microporous filter and a ferrous sulfate (FeSO4) storage tank; wherein, the outlets of the artificial rutile waste acid storage tank and the calcium carbonate suspension storage tank are connected to the inlet of the premixing tank; the outlet of the premixing tank is preferably directly connected to the inlet of the neutralization tank; the outlet of the neutralization tank, the gypsum filter press, the ferrous sulfate purification reaction tank, the sedimentation tank, the microporous filter and the ferrous sulfate (FeSO4) storage tank are connected in sequence.

[0068] In the present invention, the inventors expect to achieve efficient and continuous operation of high-quality battery-grade iron phosphate and gypsum co-production, and therefore designed an improved neutralization tank device. The neutralization tank device, premixing tank, and gypsum filter press can be combined to implement step a) in the embodiment. Figure 2 shown. Figure 2The lower half of the neutralization tank design is shown, with the upper half omitted, but the upper half of the neutralization tank may include a premixing tank connection port, an observation window, and / or a waste acid inlet, a calcium carbonate suspension inlet, and / or an acid and alkali injection port. Figure 2 As shown, the neutralization tank equipment specifically shows a tank body 1, calcium attachments 2 (calcium deposits 5 at the lower outlet) located on the side wall of the tank body, an acid-base spray port 3 extending from the lower side of the tank body 1 into the interior of the tank body 1, and a pH value monitor 6 also extending from the lower side of the tank body 1 into the interior of the tank body 1. When performing equipment operation or executing a process, the acid-base spray port 3 can select to spray sulfuric acid solution, water or calcium hydroxide solution according to the feedback data of the pH value monitor 6. The molar concentration of the sulfuric acid solution or the calcium hydroxide solution does not exceed 0.1 mol / L, preferably selected from 0.01 mol / L to 0.1 mol / L. The purpose of the acid-base spray port 3 is not to further promote the reaction of sulfuric acid and calcium carbonate to produce gypsum, but to accurately control the pH value of the liquid phase. Therefore, the spray liquid (sulfuric acid solution or calcium hydroxide solution) provided in the acid-base spray port 3 must be a dilute liquid to help control the precise pH value in the environment. In addition, the acid-base spray port 3 can rotate around its own axis to clean or remove the gypsum product attached to the tank wall while adjusting the pH value. In the present embodiment, the acid-base spray port 3 is preferably arranged at the lower part of the tank body 1, and more preferably arranged at 1 / 3 or lower of the entire height of the tank body 1 from the bottom. The pH value monitor 6 is preferably arranged at an upper position around the acid-base spray port 3, preferably directly above it, so as to timely monitor the pH value fluctuation around it when the acid-base spray port 3 sprays the corresponding liquid and timely feedback the operation of the acid-base spray port 3. In the present invention, when the reaction system is adjusted to a pH value in a suitable range by the operation of the pH value monitor 6 and the acid-base spray port 3, the outlet 7 located at the lower part can be kept in a normally open state to continuously deliver the product to the subsequent gypsum filter press. The instrument input port 4 of the equipment remains in a normally closed state, but one or more auxiliary detection devices can be inserted therein. In the embodiment of the present invention, no additional stirring equipment may be provided in the tank body 1, which not only saves equipment space, but also enables the acid-base spray port 3 to rotate around its own axis to generate a rotating spray force to achieve mixing.

[0069] The device for preparing iron phosphate and co-producing gypsum using artificial rutile waste liquid also includes a phosphate supply device. The phosphate supply device includes a diammonium phosphate dissolving tank, an ammonium salt filter press, and a pure diammonium phosphate solution storage tank connected in sequence. Preferably, the diammonium phosphate dissolving tank is also connected to ammonia water and diammonium phosphate inlets, and is also equipped with a mother liquor receiving port for receiving mother liquor returned after the preparation of the iron phosphate reaction is completed.

[0070] The device for preparing iron phosphate and co-producing gypsum using artificial rutile waste liquid also includes an iron phosphate synthesis device. The iron phosphate synthesis device includes an iron phosphate synthesis kettle, an ammonium salt metering tank, a ferrous metering tank and a hydrogen peroxide storage tank directly or indirectly connected to the iron phosphate synthesis kettle. In addition, the outlet of the iron phosphate synthesis kettle is connected to a wash filter press, a wash pulping tank, an aging kettle and an iron phosphate storage tank in sequence.

[0071] Optionally, the device for preparing iron phosphate and co-producing gypsum using artificial rutile waste liquid can also be equipped with one or more auxiliary equipment. The auxiliary equipment includes: a secondary washing filter press, a microporous filter, and a thick slurry tank connected to the outlet of the iron phosphate storage tank and arranged in sequence, and the outlet of the thick slurry tank is connected to the primary washing filter press; and / or, a regulating tank connected to the waste liquid (mother liquor) outlet of the primary washing filter press, and an inclined plate sedimentation tank connected to the regulating tank in sequence (the inclined plate sedimentation tank can also be separately connected to the high-salt wastewater filter press), a filtering device, a reverse osmosis device, and an ammonium sulfate generating device; it can also include an iron phosphate filter cake conveying device, a dryer, a rotary kiln, a steam powder machine, and a packaging machine connected to the secondary washing filter press.

[0072] Comparative Example 1

[0073] Gypsum and ferric phosphate are manufactured using the same steps as in Example 1, except that in step a), the pH value is controlled between 3.5 and 5, and the improved neutralization tank described in Example 2 is not used. Instead, a common inlet is used above the equipment to connect the acid and alkali to the neutralization tank entering the pipeline.

[0074] The inventors found that when the pH value is controlled between 3.5 and 5 or higher, in the ferrous sulfate manufacturing and co-production of gypsum equipment, it is necessary to stop the continuous operation of the equipment every half an hour to one hour of operation to clean the filter cloth of the gypsum filter press or replace the filter cloth. In contrast, in the process of Example 1, when the appropriate pH value is controlled using appropriate equipment, the ferrous sulfate manufacturing and co-production of gypsum equipment can be continuously operated for more than 24 hours without stopping. In addition, in the test of "Test Point 2" of Comparative Example 1 and Example 1, the test results in Comparative Example 1 show that the gypsum contains more than 1wt% of titanium impurities, which may be caused by the hydrolysis of Ti.

[0075] Comparative Example 2

[0076] Gypsum and iron phosphate were produced using the same steps as in Example 1, except that in step b), the pH value was controlled to be 3.5, or the pH value was controlled to be 8.

[0077] In the sample of Comparative Example 2 where the pH value was controlled to be 3.5, the Ti content in the iron phosphate product measured at test point 3 was as high as 0.1wt% to 0.3wt%, which obviously could not meet the manufacturing requirements of battery-grade iron phosphate. The inventors believe that this is because the waste acid solution with a high Ti content was used as the starting reactant in the raw material, and Ti was not fully hydrolyzed within the appropriate pH range in step b), resulting in Ti ions entering the iron phosphate product through subsequent processes under acidic synthesis conditions.

[0078] Comparative Example 3

[0079] Gypsum and iron phosphate were prepared by the same steps as in Example 1. The difference is that the improved neutralization tank provided in Example 2 was not used in the embodiment, but only a premixing tank was used as a reaction container for calcium carbonate and waste acid solution.

[0080] Through observations of industrial assembly line production, the inventors found that when only a premixing tank is used as a reaction container for calcium carbonate and waste acid liquid, it is difficult to accurately control and feedback the pH value range, which may cause the filter cloth to be blocked, or cause the calcium carbonate to fail to fully react with sulfuric acid, thereby reducing production efficiency or product yield.

[0081] In a non-limiting manner, in the process design of the inventors, the premixing step and the neutralization step are two consecutive steps. In the premixing step, sulfuric acid with a high concentration reacts quickly with calcium carbonate, and there is no need to accurately control the pH value in this step. A large amount (slightly excessive or more excessive) of sulfuric acid mixed with calcium carbonate is conducive to the formation of calcium sulfate, and the pH value at this time is far within the acidic range (far less than 1).

[0082] When the reaction in the premixing step (premixing tank) is close to the end, the connection channel between the premixing tank and the neutralization tank is opened, so that most of the products (calcium sulfate, part of calcium carbonate, sulfuric acid, etc.) after the reaction are completed enter the neutralization tank. At this time, the pH value is adjusted by a diluted calcium hydroxide solution or sulfuric acid solution, and the separation of the desired elements can be accurately and easily achieved. It can be understood that the premixing tank acts as a buffer or isolation device for the neutralization tank, so that the pH value and the separation of elements can be more accurately controlled.

[0083] In the production line practice, if high-concentration waste acid is directly reacted with a large amount of calcium carbonate powder or suspension, the reaction process is violent and it is difficult to accurately control the pH value. Especially when low-concentration calcium hydroxide or sulfuric acid solution is released in the neutralization tank, it is difficult to have an effective impact on the entire system, and it is easy to cause Ti hydrolysis or incomplete calcium carbonate reaction.

[0084] According to the implementation scheme and technical contents recorded in the specification of the present invention, the present invention can at least provide the following technical solutions: Although the present disclosure includes specific embodiments, it is obvious to those skilled in the art that various formal and detailed replacements or changes can be made to these embodiments without departing from the gist and scope of the invention of the present claims and their equivalent technical solutions. The embodiments described herein should be considered to be illustrative only and not for the purpose of limitation. The description of the features and aspects in each embodiment is considered to be applicable to similar features and aspects in other embodiments. Therefore, the scope of the present disclosure should not be limited by the specific description, but by the technical solutions of the claims, and all changes within the scope of the claims and their equivalents are interpreted as being included in the technical solutions of the present disclosure.

[0085] The present invention provides at least the following technical solutions:

[0086] Scheme 1. A method for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid.

[0087] The method comprises the following steps:

[0088] Step a): artificial rutile waste liquid and calcium carbonate suspension are pumped into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows into a neutralization tank for further neutralization reaction. During the reaction, the pH of the system is always controlled to be 2-3, and after the reaction, a ferrous sulfate solution with a pH of about 2 to 3 is obtained through a gypsum filter press;

[0089] Step b): adding the ferrous sulfate solution obtained in step a) into a ferrous sulfate purification reaction tank by a metering pump, adding a sodium hydroxide solution with a mass content to keep the solution pH at about 4 to 6, preferably adjusted to about 4 to 5, more preferably adjusted to 4 to 4.5, and heating to 70-80° C. for heat preservation; thereafter, the reaction solution is placed in a sedimentation tank, filtered through a microporous filter to obtain a purified ferrous sulfate solution and slurry, and the ferrous sulfate solution is sent to a ferrous sulfate metering tank via a ferrous sulfate storage tank;

[0090] Step c): adding ammonia water and diammonium phosphate solid (preferably, the mother liquor filtered through a microporous filter after the reaction cycle is completed) into a diammonium phosphate dissolving tank to dissolve the diammonium phosphate, and obtaining diammonium phosphate through reaction;

[0091] Step d): adding the ferrous sulfate solution in step a) into the ferric phosphate synthesis kettle, mixing the ammonium dihydrogen phosphate solution and the hydrogen peroxide solution uniformly, first pumping them into the ammonium salt metering tank, and then dripping them into the ferric phosphate synthesis kettle for reaction;

[0092] Step e): the iron phosphate obtained after the reaction in step d) is pumped into a first filter press for filtration and washing, the washed iron phosphate is slurried and pumped into an aging kettle, phosphoric acid is added into the aging kettle, and the aging is carried out for 30-90 minutes by heating; the obtained iron phosphate is further sent to a second filter press for filtration and washing to obtain an iron phosphate filter cake;

[0093] Step f): The iron phosphate filter cake obtained in step e) is sent to a dryer (such as a flash dryer) for dehydration, then calcined in a calcining kiln (such as a rotary kiln), and then crushed in a steam pulverizer to obtain battery-grade iron phosphate.

[0094] Scheme 2. The method according to Scheme 1, wherein the method further comprises:

[0095] Step g): wastewater recycling and reuse: adding ammonia water to the first wash filtrate and washing water obtained in step e) to adjust the pH value, then removing trace impurities through an inclined plate settling tank and a filtering device, the filtrate is passed through a reverse osmosis device to produce desalted water, and the desalted water is concentrated into a liquid to prepare ammonium sulfate; and

[0096] The second wash filtrate obtained in step e) is passed through a microporous filter to obtain a mother liquor, which is returned for preparing diammonium phosphate, and the washing water of the second wash step is further returned to the first wash filter press as washing water for the first wash.

[0097] Scheme 3. The method according to Scheme 1 or 2, wherein the method is carried out by the following steps:

[0098] Step a): converting the actual sulfuric acid content to the actual calcium carbonate content, and pumping the artificial rutile waste liquid with a sulfuric acid content of 8wt% to 15wt% and the calcium carbonate suspension with a calcium carbonate content of 200-400g / L into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows to a neutralization tank for further neutralization reaction, and the neutralization reaction time is 1-3 hours. After the reaction, a ferrous sulfate solution with a pH of 2 to 3 is obtained through a gypsum filter press;

[0099] Step b): adding the ferrous sulfate solution of step a) into a ferrous purification reaction tank by a metering pump, adding a sodium hydroxide solution with a mass content of about 10wt% to 20wt%, preferably adjusting the pH value of the solution to 4 to 5, more preferably to 4 to 4.5, heating to 60-85°C, keeping warm for 0.5 to 2 hours, placing in a sedimentation tank, and filtering through a microporous filter when the temperature drops below 60 degrees Celsius to obtain a purified ferrous sulfate solution and mud, the ferrous sulfate solution is sent to the next step, and the mud is sent to a sewage treatment station for treatment;

[0100] Step c): adding ammonia water with a mass concentration of 10-30wt% and diammonium phosphate solid (preferably, the mother liquor filtered through a microporous filter after the reaction cycle is completed) into a diammonium phosphate dissolving tank according to a molar ratio of the substances contained (1.0-1.1):1, dissolving the diammonium phosphate to obtain a diammonium phosphate solution. The solution is filtered through an ammonium salt filter press to obtain a pure diammonium phosphate solution.

[0101] Step d): pump the ferrous sulfate solution into the ferrous sulfate metering tank, then add it into the ferric phosphate synthesis kettle, mix the ammonium dihydrogen phosphate solution and the hydrogen peroxide solution with a mass concentration of about 20-25wt% evenly, then pump it into the metering tank, and drop it into the ferric phosphate synthesis kettle for 30-60 minutes, control the reaction temperature at 60°C, and continue the reaction for 1 hour after the dropwise addition.

[0102] Step e): The iron phosphate obtained by the reaction is pumped into a first-wash filter press for filtration and washing, and the washing is stopped when the conductivity of the washing water is ≤3500 microsiemens / cm. After the iron phosphate is slurried, it is pumped into an aging kettle, phosphoric acid is added, and it is heated to 70-90 degrees Celsius for aging for 60-120 minutes. The jacketed coil is cooled to below 55 degrees Celsius and enters a second-wash filter press for filtration and washing; the iron phosphate filter cake is sent to the next step via a belt conveyor.

[0103] Step f): The iron phosphate filter cake is first sent to a flash dryer via a screw conveyor to remove surface water, then calcined in a rotary kiln to remove crystal water, then crushed in a steam powder mill, and finally packaged to obtain battery-grade iron phosphate.

[0104] Step g): wastewater recycling and reuse: ammonia water is added to the first wash filtrate and washing water to adjust the pH in the regulating tank, and trace impurities such as organic matter are removed through the inclined plate sedimentation tank and the filtering equipment. The filtrate is passed through the reverse osmosis device to produce desalted water, and the desalted water is concentrated into liquid to produce ammonium sulfate; the second wash filtrate is passed through a microporous filter to obtain a mother liquor, which is returned for the preparation of diammonium phosphate, and the second wash water is returned to the first wash filter press as the washing water of the first wash.

[0105] Scheme 4. A method according to any one of Schemes 1 to 3, wherein the pH value of the control system in step a) is achieved by spraying a sulfuric acid solution or a calcium hydroxide solution having a molar concentration not exceeding 0.1 mol / L into the neutralization tank.

[0106] Scheme 5. The method according to any one of schemes 1 to 4, wherein the reaction in step a) is carried out by a neutralization tank, the neutralization tank comprising a tank body, an acid-base spray port extending from the lower side of the tank body into the tank body, and a pH monitor also extending from the lower side of the tank body into the tank body, the acid-base spray port selectively spraying sulfuric acid solution, water or calcium hydroxide solution according to feedback data from the pH monitor to maintain the pH of the reaction system at 2 to 3; and

[0107] The acid-base spray port is capable of rotating around its own axis and is arranged at the lower part of the trough body, more preferably, at 1 / 3 or lower of the entire height of the trough body from the bottom; the pH value monitor is preferably arranged at an upper position around the acid-base spray port, preferably at a position immediately above it.

[0108] Scheme 6. A device for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid, characterized in that the device includes ferrous sulfate production and co-production of gypsum equipment, phosphate supply equipment, iron phosphate synthesis equipment and optional auxiliary equipment; wherein:

[0109] The ferrous sulfate manufacturing and gypsum co-production equipment comprises an artificial rutile waste acid storage tank, a calcium carbonate suspension storage tank, a premixing tank, a neutralization tank, a gypsum filter press, a ferrous purifying reaction tank, a settling tank, a microporous filter and a ferrous sulfate storage tank; and the outlets of the artificial rutile waste acid storage tank and the calcium carbonate suspension storage tank are connected to the inlet of the premixing tank; the outlet of the premixing tank is preferably directly connected to the inlet of the neutralization tank; the outlet of the neutralization tank, the gypsum filter press, the ferrous purifying reaction tank, the settling tank, the microporous filter and the ferrous sulfate storage tank are connected in sequence; and

[0110] The phosphate providing equipment comprises a diammonium phosphate dissolving tank, an ammonium salt filter press and a diammonium phosphate storage tank which are connected in sequence; preferably, the diammonium phosphate dissolving tank is also connected to an ammonia water and diammonium phosphate inlet, and is also equipped with a mother liquor receiving device for receiving mother liquor returned from the iron phosphate reaction after the preparation is completed;

[0111] The ferric phosphate synthesis equipment includes a ferric phosphate synthesis kettle, an ammonium salt metering tank, a ferrous iron metering tank and a hydrogen peroxide storage tank directly or indirectly connected to the ferric phosphate synthesis kettle. In addition, the outlet of the ferric phosphate synthesis kettle is sequentially connected to a wash filter press, a wash pulping tank, an aging kettle and a ferric phosphate storage tank.

[0112] Scheme 7. An apparatus according to Scheme 6, wherein the auxiliary equipment includes a secondary wash filter press, a microporous filter, and a thick slurry tank connected to the outlet of the iron phosphate storage tank and arranged in sequence, the outlet of the thick slurry tank is connected to the primary wash filter press; and / or, a regulating tank connected to the waste liquid outlet of the primary wash filter press, and an inclined plate sedimentation tank, a filtration device, a reverse osmosis device, and an ammonium sulfate generating device connected to the regulating tank in sequence; it may also include an iron phosphate filter cake conveying device, a dryer, a rotary kiln, a steam powder machine, and a packaging machine connected to the secondary wash filter press.

[0113] Solution 8. The device according to any one of solutions 6 to 8, wherein the neutralization tank comprises a tank body, an acid-base spray port extending from the lower side of the tank body into the tank body, and a pH value monitor also extending from the lower side of the tank body into the tank body; and

[0114] The acid-base spray port can rotate around its own axis and is arranged at the lower part of the tank body, more preferably, at 1 / 3 or lower of the entire height of the tank body 1 from the bottom; the pH value monitor is preferably arranged at an upper position close to the acid-base spray port, preferably at a position immediately above it.

[0115] Embodiment 9. The device according to any one of embodiments 6 to 8, wherein the device is used for the method according to any one of embodiments 1 to 5.

[0116] Scheme 10. A scheme according to any of the preceding items, wherein the desalted water passing through the reverse osmosis device passes through a desalted water tank and enters a secondary wash filter press as wash water.

[0117] Scheme 11. A scheme according to any of the preceding items, wherein the wastewater passing through the inclined plate sedimentation tank passes through a high-salt wastewater filter press and is further subjected to sewage treatment; the resulting filter cake further enters a filtration device to filter out the desired material.

[0118] Scheme 12. A scheme according to any of the preceding items, wherein in the auxiliary equipment and / or auxiliary process, the microporous filter receives the filtrate from the secondary filter press, the filtered thick slurry is returned to the primary filter press through the thick slurry tank, and the filtered mother liquor is returned to the diammonium phosphate dissolution tank to participate in the supply of phosphate.

[0119] Solution 13. A solution according to any of the preceding items, wherein the side wall of the tank body (1) is sprayed with an acid-base spray port (3) to clean the gypsum product attached to the side wall.

[0120] Solution 14. According to any of the solutions described above, the acid-base spray port (3) is arranged at 1 / 4 or lower of the entire height of the trough body (1) starting from the bottom, and is preferably arranged at 1 / 5 or lower of the trough body.

[0121] Solution 15. According to any of the preceding solutions, no additional stirring equipment is provided in the tank body (1).

[0122] Solution 16. A solution according to any of the preceding items, wherein the straight-line distance between the end of the acid-base spray port (3) and the detection end of the pH monitor (6) does not exceed 5 cm, preferably does not exceed 3 cm, and more preferably does not exceed 1 cm.

[0123] Option 16. According to any of the preceding options, the mesh size of the filter cloth of the filter press is approximately between 150 mesh and 300 mesh, preferably selected from between 180 mesh and 250 mesh.

[0124] Scheme 17. A scheme according to any of the preceding items, wherein the reaction in step b) is carried out through the following ferrous iron purification reaction tank, the ferrous iron purification reaction tank comprising a tank body, a spray port extending from the lower side of the tank body into the interior of the tank body, and a pH monitor also extending from the lower side of the tank body into the interior of the tank body, the spray port selects spraying water or sodium hydroxide solution according to the feedback data of the pH monitor to maintain the pH of the reaction system at 4 to 6, preferably at 4 to 5 or 4 to 4.5; and the spray port is capable of rotating around its own axis and is arranged at the lower part of the tank body, more preferably, at 1 / 3 or lower of the entire height of the tank body from the bottom; the pH monitor is preferably arranged at an upper position around the spray port, preferably at a position immediately above it.

Claims

1. A method for preparing iron phosphate and co-producing white gypsum using artificial rutile waste liquid, the method comprising the following steps: Step a): artificial rutile waste liquid and calcium carbonate suspension are pumped into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows into a neutralization tank for further neutralization reaction. During the reaction, the pH of the system is controlled to be 2 to 3, and after the reaction, a ferrous sulfate solution with a pH of 2 to 3 is obtained through a gypsum filter press; Step b): adding the ferrous sulfate solution obtained in step a) into a ferrous sulfate purification reaction tank by a metering pump, adding a sodium hydroxide solution to keep the pH value of the solution at 4 to 5, and heating to 70-80° C. for heat preservation; thereafter, the reaction solution is placed in a sedimentation tank, filtered through a microporous filter to obtain a purified ferrous sulfate solution and slurry, and the ferrous sulfate solution is sent to a ferrous sulfate metering tank via a ferrous sulfate storage tank; Step c): adding ammonia water and diammonium phosphate solid into a diammonium phosphate dissolving tank to dissolve the diammonium phosphate to obtain a diammonium phosphate solution; Step d): adding the ferrous sulfate solution in step a) into the ferric phosphate synthesis kettle, mixing the ammonium dihydrogen phosphate solution obtained in step c) with the hydrogen peroxide solution, first pumping them into the ammonium salt metering tank, and then dripping them into the ferric phosphate synthesis kettle for reaction; Step e): the iron phosphate obtained after the reaction in step d) is pumped into a first filter press for filtration and washing, the washed iron phosphate is slurried and pumped into an aging kettle, phosphoric acid is added into the aging kettle, and the aging is carried out for 30-90 minutes by heating; the obtained iron phosphate is further sent to a second filter press for filtration and washing to obtain an iron phosphate filter cake; Step f): the iron phosphate filter cake obtained in step e) is sent to a dryer for dehydration, then calcined in a calcining kiln, and then crushed in a steam pulverizer to obtain battery-grade iron phosphate.

2. The method according to claim 1, wherein the method further comprises: Step g): Wastewater recycling and reuse: Ammonia water is added to the first wash filtrate and washing water obtained in step e) to adjust the pH value, and then trace impurities are removed through an inclined plate sedimentation tank and a filtration device. The filtrate is passed through a reverse osmosis device to produce desalted water, and the desalted water is concentrated into a liquid to prepare ammonium sulfate; as well as The second wash filtrate obtained in step e) is passed through a microporous filter to obtain a mother liquor, which is returned for preparing diammonium phosphate, and the washing water of the second wash step is further returned to the first wash filter press as washing water for the first wash.

3. The method according to claim 1 or 2, wherein the method is carried out by the following steps: Step a): converting the actual sulfuric acid content to the actual calcium carbonate content, and pumping the artificial rutile waste liquid with a sulfuric acid content of 8wt% to 15wt% and the calcium carbonate suspension with a calcium carbonate content of 200-400g / L into a premixing tank through a metering pump for premixing reaction, and the premixed liquid overflows to a neutralization tank for further neutralization reaction, and the neutralization reaction time is 1-3 hours. During the reaction, the pH of the system is controlled to be 2 to 3; after the reaction, a ferrous sulfate solution with a pH of 2 to 3 is obtained through a gypsum filter press; Step b): adding the ferrous sulfate solution of step a) into a ferrous purification reaction tank by a metering pump, adding a sodium hydroxide solution with a mass content of 10wt% to 20wt%, adjusting the pH value of the solution to 4 to 4.5, heating to 60-85°C, keeping warm for 0.5 to 2 hours, placing the solution into a sedimentation tank, and filtering through a microporous filter when the temperature drops below 60 degrees Celsius to obtain a purified ferrous sulfate solution and mud, the ferrous sulfate solution is sent to the next step, and the mud is sent to a sewage treatment station for treatment; Step c): adding ammonia water with a mass concentration of 10-30wt% and diammonium phosphate solid according to the molar ratio of the contained substances (1.0-1.1):1 into a diammonium phosphate dissolving tank, dissolving the diammonium phosphate to obtain a diammonium phosphate solution; and filtering through an ammonium salt filter press to obtain a pure diammonium phosphate solution; Step d): pumping ferrous sulfate solution into a ferrous sulfate metering tank, then adding it into an iron phosphate synthesis kettle, mixing the ammonium dihydrogen phosphate solution and a 20-25wt% hydrogen peroxide solution evenly, then pumping it into an ammonium salt metering tank, and then dripping it into the iron phosphate synthesis kettle, taking 30-60 minutes, controlling the reaction temperature at 60°C, and continuing the reaction for 1 hour after the dripping is completed; Step e): pumping the iron phosphate obtained by the reaction into a first-wash filter press for filtration and washing, stopping washing when the conductivity of the washing water is ≤3500 microsiemens / cm, pumping the iron phosphate into an aging kettle after pulping, adding phosphoric acid, heating to 70-90 degrees Celsius for aging for 60-120 minutes, cooling to below 55 degrees Celsius with a jacketed coil and entering a second-wash filter press for filtration and washing; the iron phosphate filter cake is sent to the next step via a belt conveyor; Step f): The iron phosphate filter cake is first sent to a flash dryer via a screw conveyor to remove surface water, then calcined in a rotary kiln to remove crystal water, then crushed in a steam pulverizer, and finally packaged to obtain battery-grade iron phosphate; Step g): Wastewater recycling and reuse: Ammonia water is added to the washing filtrate and washing water to adjust the pH in the regulating tank, and organic impurities are removed through the inclined plate sedimentation tank and filtering equipment. The filtrate is passed through a reverse osmosis device to produce desalted water, and the desalted water is concentrated into liquid to produce ammonium sulfate; The second wash filtrate is passed through a microporous filter to obtain a mother liquor, which is returned for the preparation of diammonium phosphate, and the second wash water is returned to the first wash filter press as the first wash water.

4. The method according to claim 3, wherein the pH value of the control system in the step a) is achieved by spraying a sulfuric acid solution or a calcium hydroxide solution having a molar concentration no more than 0.1 mol / L into the neutralization tank.

5. The method according to claim 4, wherein the reaction in step a) is carried out by a neutralization tank, the neutralization tank comprising a tank body, an acid-base spray port extending from the bottom of the tank body into the tank body, and a pH monitor also extending from the bottom of the tank body into the tank body, the acid-base spray port selectively spraying sulfuric acid solution, water or calcium hydroxide solution according to feedback data from the pH monitor to maintain the pH of the reaction system at 2 to 3; and The acid-base spray port can rotate around its own axis and is arranged at 1 / 3 or lower of the entire height of the tank body from the bottom; the pH value monitor is arranged at a position immediately above the acid-base spray port.

6. The method according to claim 5, characterized in that The reaction in step b) is carried out by a ferrous iron purification reaction tank, which comprises a tank body, a spray port extending from the bottom of the tank body into the tank body, and a pH value monitor extending from the bottom of the tank body into the tank body, wherein the spray port selects spray water or sodium hydroxide solution according to feedback data of the pH value monitor to maintain the pH of the reaction system at 4 to 4.5; and The spray port can rotate around its own axis and is arranged at 1 / 3 or lower of the entire height of the tank body from the bottom; the pH value monitor is arranged at an upper position around the spray port.