Method for producing nickel sulfate
By heating nickel oxide particles and aqueous acid solution in a closed pressure-resistant container, a mixture of nickel oxide dissolved is generated to prepare nickel sulfate, which solves the problem of stable supply of nickel sources, improves nickel recovery efficiency and cost-effectiveness, and is lithium ion 2 The secondary battery provides a stable nickel source.
Patent Information
- Application Number
- CN202211198286.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-04
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-09-29
AI Technical Summary
The prior art is difficult to effectively ensure the stable supply of nickel sources, especially in the case of increasing demand for nickel in the fields of lithium-ion secondary battery positive electrode active materials and stainless steel, which is a lack of efficient nickel recycling and manufacturing methods.
Heat the nickel oxide particles and an acid aqueous solution in a closed pressure-resistant container to form a mixed solution with nickel oxide dissolved, and nickel sulfate is prepared through the mixed solution, and the nickel oxide particle size, acid aqueous solution concentration and heating temperature are optimized to increase nickel. dissolution speed and production efficiency.
It realizes efficient production of nickel sulfate, improves the recycling efficiency and cost-effectiveness of nickel, provides a stable nickel source for the positive electrode active substance of lithium-ion secondary batteries, and reduces production costs.
Smart Images

Figure CN115925002B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing nickel sulfate. Background Art
[0002] In recent years, demand for lithium-ion secondary batteries has been increasing. The positive electrode active materials in lithium-ion secondary batteries are often nickel-containing materials, such as lithium-nickel-cobalt-manganese composite oxides and lithium-nickel-cobalt-aluminum composite oxides. Nickel is also used in stainless steel and special steels, and demand for these is also increasing.
[0003] Therefore, the demand for nickel has increased dramatically, and from the perspective of a stable supply of nickel sources, it is desired to develop a method for securing new nickel sources. As one of the methods for securing nickel sources, a method for recovering nickel from nickel-containing oxide ores is known (for example, see Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5060033 Summary of the Invention
[0007] The method described in Patent Document 1 is intended to ensure a nickel source for stainless steel, and therefore, nickel is ultimately obtained as ferronickel. On the other hand, nickel sulfate is generally used as a nickel source for positive electrode active materials containing nickel. Therefore, a method for producing nickel sulfate from a raw material containing nickel (such as nickel oxide) is very useful for ensuring a nickel source for positive electrode active materials of lithium ion secondary batteries.
[0008] Therefore, an object of the present invention is to provide a new method for producing nickel sulfate from nickel oxide.
[0009] The method for producing nickel sulfate disclosed herein includes: placing nickel oxide particles and an aqueous acid solution into a pressure-resistant container; heating the sealed pressure-resistant container to a temperature exceeding 100°C to obtain a mixed solution containing dissolved nickel oxide; and using the mixed solution to produce nickel sulfate. This configuration provides a novel method for producing nickel sulfate from a raw material containing nickel oxide.
[0010] In a preferred embodiment of the method for producing nickel sulfate disclosed herein, the aqueous acid solution is hydrochloric acid. This configuration increases the dissolution rate of nickel oxide in the aqueous acid solution, thereby improving the production efficiency of nickel sulfate.
[0011] In a preferred embodiment of the method for producing nickel sulfate disclosed herein, the average particle size of the nickel oxide particles is 1.0 mm or less. This configuration increases the dissolution rate of the nickel oxide in the aqueous acid solution, thereby improving the production efficiency of nickel sulfate. Furthermore, when the average particle size of the nickel oxide particles is 0.5 μm or more and 100 μm or less, the dissolution rate of the nickel oxide in the aqueous acid solution is even faster, further improving the production efficiency of nickel sulfate.
[0012] In a preferred embodiment of the method for producing nickel sulfate disclosed herein, the concentration of the aqueous acid solution is 2 mol / L or greater. Furthermore, the particles are introduced into the pressure vessel so that the concentration of nickel oxide is 0.80 mol / L or less. This configuration increases the dissolution rate of nickel oxide in the aqueous acid solution, thereby improving the production efficiency of nickel sulfate. Furthermore, when the particles are introduced so that the concentration of nickel oxide is 0.30 mol / L or greater and 0.60 mol / L or less, the dissolution rate of nickel oxide in the aqueous acid solution is further increased, further improving the production efficiency of nickel sulfate.
[0013] In a preferred embodiment of the method for producing nickel sulfate disclosed herein, the pressure vessel is heated to a temperature of 150°C to 270°C while being sealed. This configuration increases the dissolution rate of nickel oxide in the aqueous acid solution, improving the production efficiency of nickel sulfate. Furthermore, it is cost-effective. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a flow chart showing each step of the method for producing nickel sulfate of the present invention. DETAILED DESCRIPTION
[0015] The following describes embodiments of the present invention with reference to the accompanying drawings. It should be noted that matters not described in this specification but necessary for the implementation of the present invention can be understood as design matters by those skilled in the art based on prior art in the relevant field. The present invention can be implemented based on the contents disclosed in this specification and common technical knowledge in the relevant field.
[0016] Figure 1 The steps of the method for producing nickel sulfate according to the present embodiment are shown in FIG. The method for producing nickel sulfate according to the present embodiment includes: step S101 of placing nickel oxide particles and an acid aqueous solution into a pressure-resistant container (hereinafter also referred to as the "placement step"); step S102 of heating the sealed pressure-resistant container to a temperature exceeding 100°C to obtain a mixed solution containing dissolved nickel oxide (hereinafter also referred to as the "mixed solution preparation step"); and step S103 of using the mixed solution to produce nickel sulfate (hereinafter also referred to as the "nickel sulfate production step"). Each step is described in detail below.
[0017] <Input Step S101>
[0018] In the charging step S101, nickel oxide particles and an aqueous acid solution are charged into a pressure vessel. The pressure vessel can be any known pressure vessel used in chemical reactions. Specific examples include autoclaves, pressure tanks, and pressurized chambers. The pressure vessel is preferably equipped with a temperature measurement device such as a thermometer or temperature sensor.
[0019] Nickel oxide particles are commercially available and may be reagent-grade or industrial-grade.
[0020] When the particle size of the nickel oxide particles is small, the dissolution rate of the nickel oxide particles increases. In other words, if the particle size of the nickel oxide particles is large, the dissolution rate decreases. Therefore, the average particle size of the nickel oxide particles is, for example, 2.5 mm or less, preferably 1.0 mm or less, more preferably 500 μm or less, further preferably 200 μm or less, and most preferably 100 μm or less. On the other hand, if the average particle size of the nickel oxide particles is too small, it is not easy to finely grind to the desired average particle size. Therefore, the particle size of the nickel oxide particles is, for example, 0.1 μm or more, preferably 0.2 μm or more, more preferably 0.3 μm or more, and further preferably 0.5 μm or more.
[0021] In this specification, the average particle size of nickel oxide particles refers to the median diameter D50. Therefore, this average particle size can be determined, for example, by measuring a volume-based particle size distribution using a laser diffraction / scattering method, as the particle size corresponding to a cumulative frequency of 50% by volume starting from the side of the smaller particles.
[0022] The acid contained in the aqueous acid solution is not particularly limited, but inorganic acids are preferred, and examples thereof include hydrogen chloride (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), phosphoric acid (H3PO4), etc. Among them, sulfuric acid has the ability to convert the anion of nickel sulfate, namely sulfate ion (SO4 2- ) into the system. On the other hand, it is believed that hydrogen chloride can form a complex with nickel, which has the advantage of a particularly high dissolution rate of nickel oxide particles. Therefore, hydrochloric acid is preferably used as the acid aqueous solution.
[0023] The higher the acid concentration of the acid aqueous solution, the greater the dissolution rate of the nickel oxide particles. Therefore, the acid concentration of the acid aqueous solution is preferably more than 1.8mol / L (1.8M), more preferably more than 2.0mol / L. On the other hand, if the acid concentration of the acid aqueous solution is too high, it is disadvantageous in terms of cost. Therefore, the acid concentration of the acid aqueous solution is preferably below 20mol / L, more preferably below 5.0mol / L.
[0024] Regarding the amount of nickel oxide particles and the acid solution added, the smaller the amount of nickel oxide particles, the faster the dissolution rate tends to be. Therefore, it is preferred to add the nickel oxide particles and the acid solution so that the concentration of nickel oxide is 1.0 mol / L or less. The concentration of nickel oxide is more preferably 0.8 mol / L or less, and even more preferably 0.6 mol / L or less. On the other hand, if the concentration of nickel oxide is low, the output of nickel sulfate per method becomes small, which is disadvantageous in terms of cost. Therefore, the concentration of nickel oxide is preferably 0.1 mol / L or more, more preferably 0.2 mol / L or more, and even more preferably 0.3 mol / L or more.
[0025] In a preferred embodiment, the concentration of the aqueous acid solution is 2 mol / L or higher due to the high solubility of nickel oxide. Furthermore, nickel oxide particles are introduced into the pressure vessel so that the concentration of nickel oxide becomes 0.80 mol / L or lower.
[0026] There is no particular limitation on the method for adding the nickel oxide particles and the acid solution to the pressure vessel, and a known method can be used. The nickel oxide particles and the acid solution can be added to the pressure vessel either first or simultaneously.
[0027] <Mixed solution preparation step S102>
[0028] In the mixed solution preparation step S102 , the pressure-resistant container is heated to a temperature exceeding 100° C. in a sealed state to obtain a mixed solution in which nickel oxide is dissolved.
[0029] Therefore, first, the pressure-resistant container into which the nickel oxide particles and the acid aqueous solution are placed is sealed and then heated to a temperature exceeding 100°C.
[0030] Heating can be performed by a known method, for example, a method of immersing the pressure container in an oil bath for heating, a method of heating by wrapping a tape heater such as a tape heater, a film heater, a surface heater such as a silicone rubber heater around the pressure container, etc.
[0031] Nickel oxide is a poorly soluble compound and does not dissolve in the acidic aqueous solution even when heated at 100°C and normal pressure. Therefore, in this embodiment, heating is performed at a temperature exceeding 100°C. Since the pressure vessel is sealed, this heating can pressurize the interior of the pressure vessel, thereby dissolving the nickel oxide in the acidic aqueous solution. Consequently, this heating can produce a mixed solution in which the nickel oxide is dissolved in the acidic aqueous solution.
[0032] Here, the higher the heating temperature, the faster the nickel oxide dissolution rate. Therefore, the heating temperature is preferably 110°C or higher, more preferably 150°C or higher, even more preferably 180°C or higher, and most preferably 200°C or higher. However, in the high heating temperature range, the effect of increasing the nickel oxide dissolution rate becomes very small, and excessive heating leads to increased costs. Therefore, the heating temperature is not particularly limited, but is preferably 270°C or lower, and more preferably 250°C or lower.
[0033] The heating time depends greatly on the heating temperature and the type of acid. Therefore, the heating time can be appropriately selected based on the heating temperature and the type of acid to allow the nickel oxide particles to dissolve in the aqueous acid solution.
[0034] <Nickel Sulfate Production Step S103>
[0035] In the nickel sulfate production step S103, nickel sulfate is produced using the mixed solution obtained above. This step can be performed according to a known method.
[0036] When sulfuric acid aqueous solution is used as the acid aqueous solution, nickel ions and sulfate ions are present in the mixed solution. In this case, for example, the pH of the mixed solution is first adjusted using an alkaline aqueous solution (e.g., sodium hydroxide aqueous solution). The pH is preferably around 4. Then, solid-liquid separation is performed according to a known method to separate the solid phase into a liquid phase (i.e., an aqueous phase).
[0037] Nickel sulfate is crystallized from the separated aqueous phase according to a known method. The precipitated nickel sulfate can then be recovered according to a known method.
[0038] When the acid aqueous solution uses an aqueous solution of sulfuric acid, nickel ions are present in the mixed solution, but sulfate ions are not present. In this case, for example, an extractant (such as an alkyl phosphonate, etc.) is first added to the mixed solution and stirred. Then, an alkali (such as sodium hydroxide) is added to adjust the pH in a manner such that the nickel ions move to the organic phase, and the organic phase is extracted. Then, an aqueous solution of sulfuric acid is added to the extracted organic phase. Thus, the nickel ions move to the aqueous phase containing sulfuric acid. The aqueous phase is extracted, and nickel sulfate is crystallized according to a known method, and nickel sulfate can be recovered according to a known method.
[0039] In addition, depending on the use of nickel sulfate, for example, nickel sulfate may not be precipitated from the aqueous phase but may be recovered in the state of an aqueous solution.
[0040] As described above, nickel sulfate can be produced from nickel oxide particles. The method for producing nickel sulfate according to this embodiment is novel and is very useful as a new method for securing nickel sulfate used as a nickel source for positive electrode active materials in lithium ion secondary batteries.
[0041] Hereinafter, examples according to the present invention will be described, but the present invention is not intended to be limited to the contents shown in these examples.
[0042] [Example 1]
[0043] In Example 1, nickel oxide particles having an average particle size (D50) of 500 μm were used. Furthermore, nickel oxide particles having a Ni content of 75% by mass or more, an Fe content of 1% by mass or less, and an S content of 0.08% by mass or less were used.
[0044] Nickel oxide particles and 2 mol / L sulfuric acid were placed in an autoclave so that the nickel oxide concentration became 0.8 mol / L. The autoclave was sealed and heated to 110° C. using a heater.
[0045] After heating for 30 minutes, the undissolved nickel oxide particles were recovered from the mixed solution in the autoclave and their weight was determined. The weight loss confirmed that the nickel oxide particles had dissolved in the acid aqueous solution. Furthermore, the dissolution rate of the nickel oxide per 30 minutes (% / 30 minutes) was calculated based on the weight loss. This dissolution rate is shown in Table 1.
[0046] In addition, sodium hydroxide is used to adjust the mixed solution dissolved with nickel oxide to a pH of about 4. Afterwards, the liquid phase is recovered by solid-liquid separation and is put into a crystallization tank (crystallizer). A vacuum pump is used to control the internal pressure to about 7.5 kPa, and crystallization is carried out while stirring the crystallization tank with a twin-screw propeller to generate nickel sulfate. This is recovered to obtain nickel sulfate.
[0047] [Examples 2 to 12]
[0048] Nickel sulfate was obtained in the same manner as in Example 1, except that the average particle size (D50) of the nickel-containing particles, the concentration of nickel oxide, the concentration of the acid aqueous solution, and the heating temperature were changed to the values shown in Table 1. The dissolution rate of nickel oxide per 30 minutes was determined. The results are shown in Table 1.
[0049] [Examples 13 to 17]
[0050] In Examples 13 to 17, nickel oxide particles having the average particle size (D50) shown in Table 1 were used. The nickel oxide particles and 2 mol / L hydrochloric acid were placed in an autoclave to achieve a nickel oxide concentration of 0.4 mol / L. The autoclave was sealed and heated to 180°C using a heater.
[0051] After heating for 30 minutes, the undissolved nickel oxide particles were recovered from the mixed solution in the autoclave and their weight was determined. The weight loss confirmed that the nickel oxide particles had dissolved in the acid aqueous solution. Furthermore, the dissolution rate of the nickel oxide per 30 minutes was calculated based on the weight loss. This dissolution rate is shown in Table 1.
[0052] Separately, an alkylphosphonate is added as an extractant to the mixed solution in which nickel oxide is dissolved, and the mixture is stirred. Thereafter, the pH is adjusted using sodium hydroxide to allow nickel ions to migrate to the organic phase, and the organic phase is extracted.
[0053] Aqueous sulfuric acid is added to the extracted organic phase to extract the aqueous phase. The aqueous phase is placed in a crystallizer, and the pressure inside the crystallizer is controlled to approximately 7.5 kPa using a vacuum pump. Crystallization proceeds while the crystallizer is stirred with twin propellers to produce nickel sulfate. This is recovered to obtain nickel sulfate.
[0054] [Comparative Examples 1 and 2]
[0055] Nickel oxide particles and 2 mol / L sulfuric acid were placed in an autoclave to a nickel oxide concentration of 0.8 mol / L. The autoclave was sealed and heated to the temperature shown in Table 1. After heating for 30 minutes, undissolved nickel oxide particles were recovered from the mixed solution in the autoclave and their weight was determined. If there was no weight loss, the nickel oxide particles were not dissolved.
[0056] [Comparative Example 3]
[0057] Nickel oxide particles and 2 mol / L sulfuric acid were placed in an autoclave to a nickel oxide concentration of 0.8 mol / L. The autoclave was not sealed and heated to 110°C using a heater. After heating for 30 minutes, the undissolved nickel oxide particles were recovered from the mixture in the autoclave and their weight was determined. If there was no weight loss, the nickel oxide particles were not dissolved.
[0058] [Table 1]
[0059] Table 1
[0060]
[0061] As shown above, by heating nickel oxide particles and an aqueous acid solution to a temperature exceeding 100°C in a sealed pressure-resistant container, a mixed solution containing dissolved nickel oxide can be prepared, which can then be used to produce nickel sulfate. Therefore, it is clear that the production method disclosed herein can produce nickel sulfate from nickel oxide.
[0062] While specific examples of the present invention have been described in detail above, these are merely illustrative and do not limit the scope of the claims. The technology described in the claims also includes various modifications and variations of the specific examples described above.
Claims
1. A method for producing nickel sulfate, comprising: The step of placing nickel oxide particles and an acid aqueous solution into a pressure-resistant container; The step of heating the pressure-resistant container in a sealed state to a temperature of 150° C. to 270° C. to obtain a mixed solution in which nickel oxide is dissolved; and a step of using the mixed solution to generate nickel sulfate, The average particle size of the nickel oxide particles is 0.5 μm or more and 100 μm or less. The aqueous acid solution is hydrochloric acid, The particles are introduced into the pressure vessel so that the concentration of nickel oxide becomes 0.3 mol / L or more and 0.60 mol / L or less, The concentration of the acid aqueous solution is 2 mol / L or more and 20 mol / L or less, In the process of generating nickel sulfate, an extractant is added to the mixed solution, and then a base is added to adjust the pH in a manner that nickel ions move to an organic phase. After extracting the organic phase, an aqueous sulfuric acid solution is added to the extracted organic phase to move the nickel ions to an aqueous phase containing sulfuric acid, thereby extracting the aqueous phase.