Concrete antifreeze and rust-proof admixture and preparation method and application thereof

By incorporating a combination of amino-modified siloxane emulsion and alcoholamine rust inhibitor into concrete, the problem of insufficient frost resistance of concrete and insufficient rust resistance of steel bars in salt freezing environment is solved, and the durability of the structure is improved and improved. Construction is simplified.

CN115925314BActive Publication Date: 2024-10-29XINJIANG SUBOTE NEW MATERIAL CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110917232.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-11
Publication Date
2024-10-29
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively improve the frost resistance of concrete and the rust resistance of steel bars in salt-freezing environments, resulting in a shortened service life of concrete structures in cold areas. Moreover, existing hydrophobic coatings and rust inhibitors have problems such as complex construction and limited protection effects. .

Method used

A concrete anti-freeze and rust-inhibiting admixture composed of amino-modified siloxane emulsion, alcoholamine-modified polysiloxane emulsion and alcohol-amine rust inhibitor is used. The composition is incorporated into the concrete to improve the hydrophobic properties and Anti-rust properties, forming a dense adsorption layer to reduce chloride ion penetration and corrosion reactions.

Benefits of technology

It significantly improves the frost resistance of concrete and the corrosion resistance of steel bars, prolongs the service life of the structure, simplifies the construction process, and avoids coating damage and the use of toxic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003206076030000031
    Figure BDA0003206076030000031
  • Figure BDA0003206076030000051
    Figure BDA0003206076030000051
  • Figure BDA0003206076030000052
    Figure BDA0003206076030000052
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete admixtures, and in particular discloses a concrete antifreeze and rust-proofing admixture and a preparation method thereof. The concrete antifreeze and rust-proofing admixture can improve the anti-salt-freeze damage performance of concrete, effectively reduce or slow down the corrosion of steel bars in concrete, reduce the damage of chloride ions to the passivation performance of steel bar surfaces, and has no obvious effect on the performance of concrete by reasonably selecting and appropriately proportioning hydrophobic components and rust-proofing components therein, without the need for other auxiliary components such as surfactants, chelating agents or mineral micropowders. The concrete antifreeze and rust-proofing admixture has the effects of having no obvious effect on the performance of concrete, and the component proportioning is simple, which ensures that the concrete antifreeze and rust-proofing admixture can be applied to concrete to reduce the adverse effects on the performance of concrete to the greatest extent, and is particularly suitable for concrete in a salt-freeze environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of concrete admixtures, and in particular, relates to a concrete antifreeze and rust-proof admixture and a preparation method thereof, as well as an application of the admixture in concrete in a salt-freezing environment. Background Art

[0002] In northern my country, snow accumulates on the road after snowfall every winter, which can easily lead to traffic accidents and affect the normal operation of urban traffic. Deicing salt (the main component is NaCl) is usually used to remove snow from the road to ensure smooth traffic. However, the large-scale use of deicing salt leads to a high chloride ion content in the melted snow water. Once the temperature drops and the salt water freezes again, it will cause severe erosion and cracking of the concrete, that is, salt freezing damage. The degree and speed of concrete damage under salt freezing conditions are many times greater than ordinary freeze-thaw. While causing the concrete matrix to deteriorate, it will also increase the chloride ion transmission rate and increase the risk of steel corrosion. For reinforced concrete structures in cold areas, it is necessary to solve the salt freezing problem from two aspects: concrete antifreeze and steel bar rust prevention, improve the durability of the structure, and extend the service life of the reinforced concrete structure.

[0003] At present, the salt-freeze resistance of concrete matrix is ​​mainly improved by adding air-entraining agents, mineral admixtures, controlling cement dosage and water-cement ratio, but the problem of salt-freeze damage to reinforced concrete has not been solved. Studies have shown that the frost resistance of concrete is related to its internal moisture content. As the moisture content of concrete increases, the amount of freezable water inside the matrix increases during the cooling process, and the degree of damage increases; therefore, the water absorption rate of concrete can be reduced through hydrophobic technology, the amount of freezable water inside the concrete is reduced, and the degree of damage during the freeze-thaw process is further reduced, thereby improving the frost resistance of concrete.

[0004] There are two main ways to improve the hydrophobicity of concrete and reduce water absorption: overall hydrophobicity of concrete and surface coating. The surface coating of concrete is to achieve the purpose of hydrophobicity by applying a layer of hydrophobic material on the surface of the substrate to isolate the concrete substrate from water; however, the common problem of coating materials is that during use, the coating will be damaged due to abrasion and other damage, thereby weakening the protective effect on concrete. In addition, the surface film-forming coating has a relative deformation due to the difference in thermal and mechanical changes between the film-forming material and the concrete itself, which affects its service life. At present, many reports on hydrophobic coatings generally have problems such as complex construction process, lack of verification of the long-term antifreeze performance of concrete and coating life. The overall hydrophobicity of concrete is to make the concrete have a certain hydrophobic ability by adding hydrophobic materials into the substrate. The more commonly used internal hydrophobic materials include silanes, nano-silicones, etc. The hydrophobicity of overall hydrophobic concrete is generally less affected by external factors and has the same life cycle as concrete.

[0005] Chloride ions can destroy the oxide passivation film on the surface of steel bars, causing the steel bars to rust and age rapidly. The volume of steel bar corrosion products expands, causing concrete cracking, affecting the strength and quality of reinforced concrete structures. The corrosion resistance of steel bars can be improved by adding reinforced concrete rust inhibitors. Reinforced concrete rust inhibitors refer to chemical substances that are added to concrete or applied to the concrete surface to prevent or slow down the corrosion of steel bars. Nitrite-based anticorrosion rust inhibitors were widely used in the early days. The disadvantage of such rust inhibitors is that they are toxic and have different degrees of negative impact on the setting time, early strength and later strength of concrete. Currently, organic rust inhibitors are widely used, mainly including alcohol amines and imidazolines. Organic steel bar rust inhibitors can utilize the porous structure of concrete to diffuse between the pores of concrete to reach the surface of steel bars, forming an effective protective film, thereby preventing the free diffusion of substances related to corrosion reactions at the steel bar / concrete interface, and achieving the effect of inhibiting corrosion. Therefore, it is considered to delay the corrosion of steel bars caused by chloride ions in concrete by using steel bar rust inhibitors in salt-freezing environments.

[0006] By improving the antifreeze performance of concrete with hydrophobic materials and the antirust performance of steel bars with rust inhibitors, the concrete matrix and steel bars are protected in salt-freeze environments. Improving the anti-salt-freeze damage performance of reinforced concrete structures and extending the service life of the structures are new directions for the protection of reinforced concrete in salt-freeze environments.

[0007] At present, there are many reports on improving the performance of reinforced concrete in salt-freezing environment from the two perspectives of hydrophobic materials and rust inhibitors. For example, a surface coating with anti-salt-freezing and anti-rust functions is prepared with raw materials such as silane, isobutyl silane, octyl silane or isooctyl silane, triethanolamine, polyoxyethylene ether non-ionic surfactant, boric acid, etc. to prepare a coating stock solution. After being applied to the concrete surface, the concrete has certain hydrophobic and anti-permeability properties and steel bar rust prevention functions, thereby improving the ability of concrete components to resist salt-freezing; however, this surface coating increases the construction process during use, and the penetration depth of the coating in the concrete matrix is ​​limited. Once the coating is worn and damaged, the protective effect on the concrete is weakened. Another example is a composite waterproofing agent for salt-freezing resistance of low-strength grade concrete, whose main components include sulphoaluminate cement, anhydrite component, mineral powder, air-entraining component, water-retaining component, hydrophobic component and retarding component, wherein the mineral powder is composed of three mineral admixtures: ultrafine fly ash, mineral powder and fly ash; the air-entraining component is composed of triterpenoid saponin air-entraining agent; the water-retaining component is composed of cellulose ether or white dextrin; the hydrophobic component is composed of organosilicon powder; and the retarding component is composed of sodium hexametaphosphate; however, this technology uses powder materials such as ultrafine fly ash, mineral powder and fly ash, which may affect the working performance of concrete during use, and the effect of organosilicon powder on improving the hydrophobicity of concrete is limited.

[0008] Therefore, it is necessary to develop a new type of concrete antifreeze and rust inhibitor to meet the needs of improving the antifreeze performance of concrete and the rust resistance of steel bars in salt-freezing environments. Summary of the invention

[0009] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to develop an additive-type concrete antifreeze and rust-proof admixture for salt-freeze environments, which can not only improve the concrete's resistance to salt-freeze damage, but also effectively reduce or slow down the corrosion of steel bars in concrete, reduce the damage of chloride ions to the passivation performance of the steel bar surface, and has no obvious effect on the concrete performance.

[0010] The technical solution for implementing the present invention is as follows:

[0011] A concrete antifreeze and rust-proof admixture, which is composed of the following components expressed in mass percentage and mixed evenly:

[0012]

[0013] Among them, the hydrophobic component can be any one of amino-modified silicone emulsion, alcoholamine-modified polysiloxane emulsion, and amino-modified polyether polysiloxane emulsion, or a combination of at least two of them, and the rust-inhibiting component can be any one of diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, and triisopropanolamine, or a combination of at least two of them.

[0014] At least one of amino-modified silicone emulsion, amine-modified polysiloxane emulsion, and amino-modified polyether polysiloxane emulsion is used as the main hydrophobic component in the concrete antifreeze and rust-resistant admixture because they can accelerate cross-linking in an alkaline environment to form a composite complex product. This type of product has high permeability and airtightness, and has a good filling effect on the pores of inorganic materials, thereby improving the hydrophobic performance of concrete.

[0015] At least one of diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine and triisopropanolamine is used as the rust-inhibiting component in the concrete antifreeze and rust-inhibiting admixture. The alcoholamine rust inhibitor is selected to show better performance in compatibility and rust-inhibiting efficiency than conventional rust inhibitors such as nitrites, molybdates, phosphates, carboxylates, quaternary ammonium salts and the like. The invention avoids the disadvantages of nitrites and molybdates being toxic to human body and environment, the problem of phosphates causing microbial enrichment and the technical difficulty that carboxylates and quaternary ammonium salts have poor compatibility with siloxane and require other auxiliary components such as surfactants or mineral micropowders or chelating agents.

[0016] In the concrete antifreeze and rust-proof admixture of the present invention, the anti-corrosion performance of the steel bars when applied to reinforced concrete is improved by the rust-proof components. Specifically, the rust-proof molecules have a good adsorption effect on the steel bar matrix, and can form a dense adsorption layer on the surface of the steel bars. The rust-proof molecules cover the surface of the steel bars in an interlaced manner, reducing the penetration of harmful ions in the environment to the surface of the steel bars; on the other hand, the rust-proof molecules can effectively inhibit the redox reaction of corrosion on the surface of the steel bars, thereby effectively increasing the critical chloride ion concentration of the steel bars and delaying the occurrence of steel bar corrosion. Under the combined effect of these two mechanisms, it is ensured that the concrete antifreeze and rust-proof admixture can improve the corrosion resistance of the steel bars and extend the service life of the steel bars.

[0017] The hydrophobic component in the present invention adopts a modified siloxane emulsion. By modifying the siloxane, the rust-inhibiting component is helped to dissolve in the hydrophobic component, thereby having good solubility; the rust-inhibiting component can be directly dissolved in the hydrophobic component by stirring, which is a simple method. Reducing the use of other components not only helps to reduce costs, but also reduces other problems caused by complex mixing, such as slow setting and reduced working performance.

[0018] Furthermore, the air entraining component may be any one of a modified rosin soap air entraining agent, a saponin air entraining agent, an alkyl sulfonate air entraining agent, an alkyl sulfate air entraining agent, or a combination of at least two thereof.

[0019] Generally speaking, the water component in the concrete antifreeze and rust-resistant admixture can be municipal tap water.

[0020] The preparation method of the above concrete antifreeze and rust-resistant admixture of the present invention can be prepared by the following steps: the hydrophobic component, the rust-resistant component and the air-entraining component are uniformly dispersed in water according to the above mass ratio to obtain the concrete antifreeze and rust-resistant admixture.

[0021] The concrete antifreeze and rust-proofing admixture provided by the present invention can be applied to concrete, and is particularly suitable for use in salt-freezing environments. Specifically, during the concrete mixing process, the concrete antifreeze and rust-proofing admixture is added thereto, and the mixing water for the concrete is deducted accordingly according to the water content of the added concrete antifreeze and rust-proofing admixture.

[0022] Generally speaking, the amount of concrete antifreeze and rust-resistant admixture added can be controlled to be 5% to 25% of the mass of the cementitious material in the pre-prepared concrete.

[0023] Beneficial effects of the present invention:

[0024] 1. The concrete antifreeze and rust-proof admixture provided by the present invention is particularly suitable for use in salt-freezing environments. It can not only effectively improve the frost resistance of concrete, but also prolong the freeze-thaw damage time and the damage of chloride ions to the passivation performance of the steel bar surface, thereby prolonging the time for chloride ions to induce steel bar corrosion.

[0025] 2. The preparation method of the concrete antifreeze and rust-resistant admixture of the present invention is simple. It only needs to add the set proportions of each group directly into water to dissolve and mix. At the same time, the amount of water used in the corresponding concrete molding process can be deducted when used. It is easy to use and does not require additional steps. The concrete antifreeze and rust-resistant admixture in liquid form provided by the present invention can effectively avoid the adverse effects on the uniformity of non-liquid products due to vibration and the like during transportation.

[0026] 3. The concrete antifreeze and rust-proofing admixture of the present invention can be widely used in buildings in cold areas where deicing salt is used, as well as in northern marine areas. DETAILED DESCRIPTION

[0027] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and the various modifications suitable for specific intended applications.

[0028] The embodiments of the present invention provide specific compositions and proportions of a number of concrete antifreeze and rust-proof admixtures. At the same time, in order to demonstrate the good effects of antifreeze and rust-proofing when applied in concrete, each concrete antifreeze and rust-proof admixture is added thereto according to the mix proportion standard of C40 concrete in Table 1 below, and the water absorption performance, salt freezing performance and electrochemical performance of the obtained concrete are measured.

[0029] Table 1C40 concrete mix ratio (kg / m 3 )

[0030]

[0031] The following Table 2 shows the specific composition and proportion of various concrete antifreeze and rust-proof admixtures provided in various embodiments of the present invention, as well as the dosage of each concrete antifreeze and rust-proof admixture applied to the C40 concrete shown in the above Table 1; the following dosages all refer to the percentage of the concrete antifreeze and rust-proof admixture in the mass of the cementitious material in the C40 concrete.

[0032] Table 2 Components and dosage of concrete antifreeze and anti-rust admixtures in Examples 1 to 14

[0033]

[0034]

[0035] The concrete antifreeze and rust-proof admixtures in the above-mentioned embodiments were applied to C40 concrete, and the concrete water absorption rate was tested after the concrete was cured to 7 days. The salt-freeze resistance of the concrete was tested when the concrete was cured to 28 days. After 56 salt-freeze cycles, the steel bar electrochemical test was carried out to determine the steel bar corrosion condition.

[0036] At the same time, in order to reflect the effects of the above-mentioned concrete antifreeze and rust-proof admixtures provided by the present invention, the C40 concrete shown in Table 1 above is used as a blank control example, and the same method as above is used to measure the various properties at the same age.

[0037] Specifically, after the concrete is cured to the specified age, the water absorption rate of the concrete is tested according to the water absorption rate method in JC / T 2553-2019 "Concrete Anti-corrosion Inhibitors" to verify the concrete's hydrophobicity. The smaller the water absorption rate, the stronger the concrete's hydrophobicity, and vice versa.

[0038] After the concrete is cured to the specified age, a salt freezing test is carried out according to the single-sided freeze-thaw method (salt freezing method) in GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" to verify the salt freezing resistance of concrete in different groups. After the concrete is salt frozen 56 times, its spalling mass and relative dynamic modulus are tested. The spalling mass and relative dynamic modulus of concrete represent the strength of the concrete's salt freezing resistance. Under the same number of freeze-thaw cycles, the smaller the spalling mass and the larger the relative dynamic modulus, the better the concrete's salt freezing resistance.

[0039] During the concrete forming process, the treated steel bars are embedded in the concrete and connected by wires. After the concrete is cured to the specified age, it is immersed in a 3% NaCl solution for three months. Three months later, the corrosion potential and corrosion current density of the steel bars are tested by an electrochemical workstation, and the corrosion condition of the steel bars in the concrete is judged according to the evaluation criteria in GB / T33803-2017 "Technical Specifications for the Application of Corrosion Inhibitors for Reinforced Concrete". It is generally believed that when the corrosion potential is greater than -200mV, the steel bars have no corrosion activity or the corrosion activity is uncertain, and the probability of corrosion is 5%; when the corrosion potential is in the range of -200mV to -350mV, the probability of steel bars corroding is 50%; when the corrosion potential is in the range of -350mV to -500mV, the probability of steel bars corroding is 95%. Similarly, the corrosion state of the steel bars can be judged according to the size of the apparent corrosion current density: when the apparent corrosion current density is less than 0.2μA / cm 2 When the apparent corrosion current density is 0.2μA / cm 2 ~0.5μA / cm 2 When the apparent corrosion current density is 0.5μA / cm 2 ~1.0μA / cm2 When the apparent corrosion current density is greater than 1.0 μA / cm 2 When the steel bar is at a high corrosion rate, the corrosion state of the steel bar can be used to determine the anti-rust effect of the admixture.

[0040] The test results of the performance of the concrete antifreeze and rust-resistant admixtures provided in the above-mentioned Examples 1 to 14 and Comparative Examples 1 to 3 when applied and the various properties of the blank comparative examples are shown in Table 3 below.

[0041] Table 3 Application performance of concrete antifreeze and rust-proof admixtures in Examples 1 to 14, Comparative Examples 1 to 3 and performance of blank comparative examples

[0042]

[0043]

[0044] By comparing the comparative example 1 with the example 1 in Table 3, it can be found that if the hydrophobic component defined in the concrete antifreeze and rust-proofing admixture of the present invention is not used, the 7d water absorption rate of the corresponding concrete is significantly increased, and the spalling quality is increased, indicating the necessity of selecting a specific hydrophobic component in the concrete antifreeze and rust-proofing admixture of the present invention. At the same time, since the rust-proofing component cannot be effectively dissolved in the hydrophobic component, the rust-proofing component in the concrete cannot be evenly distributed, and the potential difference generated at different positions accelerates the corrosion of the steel bars, resulting in an increase in the test half-cell potential and corrosion current. The comparison between comparative example 2 and example 2 verifies the necessity of the rust-proofing component in the concrete antifreeze and rust-proofing admixture of the present invention. It can be found from the test results that if the rust-proofing component required in the invention is not used, the half-cell potential and corrosion current density of the steel bars in the concrete are significantly increased, indicating that the risk of steel bar corrosion in the concrete is serious and the protective effect on the steel bars is weak. By comparing comparative example 3 with example 3, it can be seen that the air entraining component in the concrete antifreeze and rust-proofing admixture of the present invention has a beneficial effect on reducing the quality of concrete salt freezing spalling in applications.

[0045] By comparing the 7d water absorption of the concrete obtained in the corresponding embodiments in Table 3 with the concrete in the blank control example, it can be seen that the concrete in the blank control example that does not use the concrete antifreeze and rust-resistant admixture provided by the present invention has a 7d water absorption of 1.82%, while the concrete to which the concrete antifreeze and rust-resistant admixtures in Examples 1 to 14 of the present invention are added has a significantly reduced 7d water absorption. The water absorption of the concrete antifreeze and rust-resistant admixtures corresponding to each embodiment is generally reduced by more than 50%, proving that the concrete antifreeze and rust-resistant admixture plays an excellent role in hydrophobicity.

[0046] By comparing the spalling mass and relative dynamic elastic modulus of the concrete obtained in the corresponding embodiments in Table 3 with the concrete in the blank control example, it can be seen that the spalling mass of the concrete to which the concrete antifreeze and rust-resistant admixtures in Examples 1 to 14 of the present invention are added is greatly reduced compared with that in the blank control example, while the relative dynamic elastic modulus is greatly improved compared with that in the blank control example, indicating that the concrete antifreeze and rust-resistant admixtures provided in the embodiments of the present invention can have good salt-freeze resistance.

[0047] By comparing the half-cell potential and corrosion current density of the concrete obtained in each embodiment in Table 3 with the concrete in the blank comparative example, it can be seen that when the half-cell potential of the concrete in the blank comparative example is -365mV, the apparent current density has reached 1.75μA / cm 2 , at this time, the steel bars in the concrete have been corroded; except for Example 2, the battery potential of the steel bars in the other groups is less than -200mV, and the corrosion current density is less than 0.1μA / cm 2 , indicating that the steel bar is in a passivated state at this time, proving that the concrete antifreeze and rust-proof admixture provided by the present invention plays an important role in steel bar rust prevention.

[0048] While the invention has been shown and described with reference to the particular embodiments, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the invention as defined by the claims and their equivalents.

Claims

1. A concrete antifreeze and rust-proof admixture, characterized in that: It is composed of the following components expressed in mass percentage which are mixed evenly: Hydrophobic component 5%~15%; Rust-inhibiting component 5%~10%; Air entrainment component 0.05%~0.5%; Water 65%~90%; The total mass percentage of the hydrophobic component, the rust-inhibiting component, the air-entraining component and water is 100%; Among them, the hydrophobic component is selected from at least one of amino-modified silicone emulsion, alcoholamine-modified polysiloxane emulsion, and amino-modified polyether polysiloxane emulsion, the rust-inhibiting component is selected from at least one of diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, and triisopropanolamine, and the air-entraining component is selected from at least one of saponin air-entraining agents, alkyl sulfonate air-entraining agents, and alkyl sulfate air-entraining agents.

2. The concrete antifreeze and rust-proof admixture according to claim 1, characterized in that: The water is municipal tap water.

3. The method for preparing the concrete antifreeze and rust-proof admixture according to claim 1 or 2, characterized in that: The method comprises the following steps: uniformly dispersing a hydrophobic component, a rust-inhibiting component and an air-entraining component in water according to a mass ratio to obtain a concrete antifreeze and rust-inhibiting admixture.

4. The use of the concrete antifreeze and rust-proof admixture according to claim 1 or 2, characterized in that: During the concrete mixing process, the concrete antifreeze and rust-resistant admixture is added thereto, and the mixing water of the concrete is deducted accordingly according to the water content in the concrete antifreeze and rust-resistant admixture.

5. The use according to claim 4, characterized in that: The added amount of the concrete antifreeze and rust-proof admixture is 5% to 25% of the mass of the cementitious material in the concrete.

Citation Information

Patent Citations

  • Water-proof corrosion inhibitor and preparation method thereof

    CN101269932A

  • Composite anti-corrosive rust inhibitor for preparing high-durability concrete

    CN101412601A

  • Concrete preservative

    CN102126842A

  • Compound concrete anti-corrosion and rust-resistant agent

    CN104478286A

  • Salt-frost-resistant and rust-resistant coating for concrete member