A modified soybean protein nonwoven fabric and preparation method thereof
Through graft modification and gel spinning technology of soy protein fiber, soy protein non-woven fabrics with high strength and wear resistance are prepared, which solves the shortcomings of traditional soy protein fiber in industrial production and achieves environmental protection, Low cost and high performance nonwoven material.
Patent Information
- Application Number
- CN202211207877.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-30
AI Technical Summary
In industrial production, traditional soybean protein fiber has problems such as less curl, low curl fastness, poor abrasion resistance, easy pilling, high water absorption, insufficient wet spinning strength, and the fabric is prone to shrinkage and deformation.
By grafting and modifying pure natural soy protein isolate and using gel spinning to prepare non-woven materials, the prepared modified soy protein non-woven fabric has unique excellent processing properties, high strength, friction resistance, and can Resistant to microbial attack.
It achieves the high strength, friction resistance and biological safety of the modified soy protein non-woven fabric, and is environmentally friendly, easily degradable and low-cost. It is suitable for environmental protection, clothing, medical beauty and other fields.
Smart Images

Figure CN115928317B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of degradable fiber materials, and in particular relates to a modified soybean protein nonwoven fabric and a preparation method thereof, and belongs to the field of functional composite materials. Background Art
[0002] Non-woven fabric is a kind of fabric that does not need spinning and weaving, but is directly bonded together by physical methods, so it is impossible to extract the thread from it. It breaks through the traditional textile principle. Compared with traditional pure cotton textiles, non-woven fabrics have the advantages of moisture-proof, breathable, flexible, light, non-combustible, easy to decompose, non-toxic and non-irritating, low price, recyclable and reuse, and have a wide range of applications. In medicine, it can be used to produce masks, surgical caps, disposable surgical gowns, disposable medical sheets, diapers, etc.; in agriculture, it can be used for harvest cloth, greenhouse cloth, etc.; in packaging, it can be used for composite cement bags, luggage linings, packaging base linings, etc.; household clothing can be used for sofa inner cloth, shopping bags, sleeping bags, etc. Traditional non-woven materials are mainly made of petrochemical fibers (such as polypropylene). With the increasingly depleted oil resources and the incomplete or even indegradable environmental pollution problems, people gradually turn their attention to environmentally friendly biodegradable raw materials.
[0003] Soy protein fiber fabrics have the characteristics of luxurious appearance, good comfort, good dyeability, etc., because of their good affinity with human skin and contain a variety of essential amino acids for the human body, they have good health care effects. At present, the development of soybean protein fiber is mainly concentrated in high-end knitted inner and outer garments, shirts, close-fitting clothing fabrics, home textile fabrics, etc., which is bound to bring new opportunities for the development of the textile industry. Although pure soybean protein fiber has many advantages, it also has some shortcomings, such as: soybean protein fiber single spinning has less curling, low curling fastness, poor wear resistance, easy pilling, high water absorption, insufficient wet spinning strength, and easy shrinkage and deformation of the fabric in industrial production. Summary of the invention
[0004] In view of the above-mentioned shortcomings, the purpose of the present invention is to provide a modified soybean protein non-woven fabric and a preparation method thereof, wherein pure natural soybean protein isolate is grafted and modified and then prepared into a non-woven fabric material by gel spinning; the prepared modified soybean protein non-woven fabric has unique excellent processing performance, high strength, and friction resistance, and is not easy to react to external effects, can resist microbial erosion, and at the same time has biosafety, is environmentally friendly and easy to degrade, has low cost, abundant raw materials, greater research significance, and more potential for development prospects.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a modified soybean protein non-woven fabric, comprising the following steps:
[0006] Step 1: Take the following components by mass: 92-98 parts of modified soybean protein fiber, 1-4 parts of softener, and 1-4 parts of stabilizer;
[0007] Step 2: adding a softener to the modified soybean protein fiber in sterile water at 30-60° C., preserving and softening for 12-24 hours, and then breaking the softened fiber by ultrasound to obtain ultra-short fibers;
[0008] Step 3: Lay the ultrashort fibers on a fiber web template, oscillate ultrasonically at 80-100 kHz for 10-30 minutes, let settle for 10-30 minutes, and repeat 3-5 times to obtain a modified soybean protein fiber web;
[0009] Step 4: Add stabilizer and then vacuum to 5x10 -8 Pa, keep warm for 120-180 minutes, then return to 45-50℃ and normal pressure for standby use;
[0010] Step 5: hydroentangle the fiber web to obtain a hydroentangled modified soybean protein fiber web; wash the hydroentangled modified soybean protein fiber web with sterile water, dry, cut and package to obtain a modified soybean protein non-woven fabric.
[0011] As a preferred embodiment of the above technical solution, in step 1, the softening agent is one or more of sulfonated oil, castor oil, birch bark tar and silicone oil.
[0012] As a preferred embodiment of the above technical solution, in step 1, the stabilizer is any one or more of phosphite, rosin acid, polyol, and tall oil.
[0013] As a preferred embodiment of the above technical solution, in step 2, the ultrasonic fragmentation frequency is 100-150 kHz and the time is 30-60 min.
[0014] As a preferred embodiment of the above technical solution, in step five, during the hydroentanglement treatment, the water pressure is 30-60 kPa, the front side is sprayed for 5-15 minutes, the back side is sprayed for 3-5 minutes, and the front and back sides are alternated for 5-15 times.
[0015] As a preferred embodiment of the above technical solution, the modified soybean protein fiber in step 1 is prepared as follows:
[0016] 1) Take the following components by mass: 92-98 parts of modified soybean protein, 1-4 parts of softener, and 1-4 parts of stabilizer;
[0017] 2) dissolving the mixture in step 1) in a solvent according to the proportion, continuously dispersing by ultrasonication for 1 to 2.5 hours until the solution is uniform, and obtaining a spinning solution with a concentration of 5 to 30 wt % after degassing at 30 to 50° C.;
[0018] 3) The spinning solution is ejected from the spinneret with an aperture range of 0.06 to 0.15 mm, and the nascent fiber is obtained by passing through an air cooler at 10 to 30°C, and the initial gel fiber is obtained by cooling in a water bath at 2 to 10°C;
[0019] 4) extracting the initial gel fiber in an extractant for 20 to 60 minutes, drying the extracted initial gel fiber at a temperature of 40 to 70° C. for 8 to 24 hours to volatilize excess extractant;
[0020] 5) The obtained primary fiber is subjected to heat stretching and shaping to obtain modified soybean protein fiber.
[0021] As a preferred embodiment of the above technical solution, in step 2), the softening agent is one or more of sulfonated oil, castor oil, birch bark tar and silicone oil.
[0022] As a preferred embodiment of the above technical solution, in step 2), the stabilizer is any one or more of phosphite, rosin acid, polyol, and tall oil.
[0023] As a preferred embodiment of the above technical solution, in step 2), the solvent is one or more of N,N-dimethylformamide, acetone, ether, and tetrahydrofuran, and the ultrasonic degassing frequency is 30 to 50 kHz.
[0024] As a preferred embodiment of the above technical solution, in step 4), the extractant is one or more of acetone and tetrahydrofuran.
[0025] As a preferred embodiment of the above technical solution, in step 5), the heat stretching and shaping is specifically performed under the conditions of heat stretching temperature of 60 to 120° C., stretching multiple of 5 to 30 times, and heat setting time of 3 to 20 minutes.
[0026] As a preferred embodiment of the above technical solution, the modified soy protein is prepared as follows:
[0027] 1.1) Add soy protein isolate and urea solution into a reactor, stir for 1 to 1.5 hours in a water bath at 30 to 50°C under nitrogen flow, adjust the pH to 8 to 10 with sodium hydroxide, then raise the temperature to 60 to 90°C and react for 1 to 2 hours to allow the protein molecules to fully stretch in the solution and open the disulfide bonds;
[0028] 1.2) Adjust the water bath temperature to 50-80°C, add the initiator after the temperature stabilizes, stir for 10-20 minutes, slowly drop the reaction grafting monomer, control the drop time to 30-50 minutes, the stirring speed to 150-200 rpm, and set the grafting time to 2-6 hours;
[0029] 1.3) The sample solution is allowed to stand and precipitate, and after filtering the precipitate, it is repeatedly washed with water for 3 to 5 times to remove unreacted inorganic salts. After filtering, it is placed in a vacuum drying oven and evacuated to 100 to 150 Pa, and dried at 50 to 80° C. for 12 to 48 hours to obtain modified soy protein.
[0030] As a preferred embodiment of the above technical solution, in the step 1.1), the mass ratio of the soy protein isolate to the urea solution is 1:2 to 1:10, and the concentration of the urea solution is 2 to 8 mol / L.
[0031] As a preferred embodiment of the above technical solution, in step 1.2), the initiator is one or a mixture of sodium sulfite, ammonium persulfate, cerium ammonium nitrate, ferrous sulfate, sodium bisulfite, ammonium ferrous sulfate, thiourea, and ascorbic acid.
[0032] As a preferred embodiment of the above technical solution, in the step 1.2), the grafting monomer is one or a mixture of methacrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and hexyl methacrylate.
[0033] A modified soybean protein nonwoven fabric prepared by any of the above preparation methods, wherein the modified soybean protein nonwoven fabric has an elongation at break of 1.2-2.0 GPa, a Young's modulus of 15-20 GPa, and an elongation at break of 8-12%.
[0034] Compared with the prior art, the advantages of the present invention are: the modified soybean protein non-woven fabric material prepared by grafting modified soybean protein isolate not only has the advantages of low cost, abundant raw materials and environmentally friendly and degradable traditional soybean protein non-woven fabric, but also has unique excellent processing performance, high strength, friction resistance, and is not easy to react to external effects and can resist microbial erosion. It can be applied to environmental protection, clothing, medical beauty, daily necessities and other fields, and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.
[0036] Figure 1 The present invention is a schematic diagram of the gel spinning process of a modified soybean protein fiber material. DETAILED DESCRIPTION
[0037] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.
[0038] Figure 1 The present invention is a schematic diagram of a gel spinning process of a modified soybean protein fiber, and the gel spinning process includes:
[0039] (1) Inject the spinning solution 1 into the hopper 2, and introduce nitrogen into the nozzle 3, and connect the metering pump 4, the motor 5, and the speed regulator 6;
[0040] (2) starting the metering pump 4 to extrude the spinning solution 1, setting the aperture range to 0.06-0.15 mm, the temperature range of the air cooler 7 to 10-30° C., and the temperature range of the water bath condenser 8 to 2-10° C.;
[0041] (3) The obtained primary gel fiber 10 is placed in an extraction tank 9 for extraction and then left to dry, the extraction temperature is 10-30° C., the time is 20-60 min, the drying temperature is 40-70° C., and the drying time is 8-24 h;
[0042] (4) Heat stretching and shaping is performed under the conditions of a heat stretching temperature of 60 to 120° C., a stretching ratio of 5 to 30 times, and a heat setting time of 3 to 20 minutes.
[0043] Example 1
[0044] 1) In a nitrogen atmosphere, the soy protein isolate was dispersed in a 2.4 mol / L urea solution. The mixture was stirred for 1.5 h in a 35°C water bath, adjusted to pH=8 with a sodium hydroxide solution, and then heated to 85°C and reacted for 1 h to activate the soy protein isolate.
[0045] 2) Adjust the grafting reaction temperature to 70°C, add ammonium persulfate and sodium bisulfite after the temperature stabilizes, stir for 10 minutes, add methyl methacrylate dropwise, and the grafting reaction time is 4 hours. Generate a water-insoluble copolymer product, remove the product, wash it repeatedly, and vacuum dry it to complete the grafting modification of soy protein isolate and obtain modified soy protein.
[0046] 3) Components and mass ratio:
[0047] Modified soy protein: 92 parts;
[0048] Sulfonated oil: 4 parts;
[0049] Phosphite: 4 parts
[0050] 4) dissolving the modified soybean protein in N,N-dimethylformamide according to the ratio, continuously dispersing by ultrasonic for 2.5 hours until the solution is uniform, and then keeping the solution warm and standing to degas to obtain a spinning solution with a concentration of 25 wt%;
[0051] 5) The spinning solution was ejected from a 0.1 mm spinneret, cooled in a 10° C. air cooler and a 5° C. water bath to obtain nascent fibers, and then the nascent fibers were extracted with an acetone solvent at a temperature of 10° C. for 30 min, dried at 50° C. for 24 h, and then heat-stretched and shaped at a heat-stretching temperature of 60° C., a stretching multiple of 10 times, and a heat-setting time of 10 min to obtain modified soybean protein fibers;
[0052] 6) Components and mass ratio:
[0053] Modified soy protein fiber: 95 parts
[0054] Sulfonated oil: 1 part
[0055] Castor oil: 3 parts
[0056] Phosphite: 1 part
[0057] 7) adding the prepared modified soybean protein fiber, sulfonated oil and castor oil to 60° C. sterile water, keeping warm and softening for 24 hours, and then breaking the softened fiber by 150 kHz ultrasound to obtain ultra-short fibers;
[0058] 8) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 80 kHz for 30 minutes, settling for 10 minutes, repeating this process three times to obtain a modified soybean protein fiber web;
[0059] 9) Add phosphite and then vacuum to 5x10 -8 Pa, keep the temperature for 120 min, then return to 50 °C and normal pressure for standby use;
[0060] The fiber web was subjected to hydroentanglement treatment at a water pressure of 30 kPa, with the front side sprayed for 5 minutes and the back side sprayed for 3 minutes, alternating between the front and back sides for 15 times, to obtain a hydroentangled modified soybean protein fiber web;
[0061] 10) The spunlace modified soybean protein fiber web is washed with sterile water, dried, cut and packaged to obtain a modified soybean protein non-woven fabric.
[0062] Example 2
[0063] 1) Disperse soy protein isolate in 3.5 mol / L urea solution under nitrogen atmosphere. Stir for 1.5 h in a 35°C water bath, adjust pH to 8 with sodium hydroxide solution, heat to 85°C, react for 1.5 h, and activate the soy protein isolate.
[0064] 2) Adjust the grafting reaction temperature to 75°C, add potassium persulfate and anhydrous sodium sulfite after the temperature stabilizes, stir for 10 minutes, add methyl methacrylate as the grafting monomer, and the grafting reaction time is 5 hours. Generate a water-insoluble copolymer product, remove the product, wash it repeatedly, and vacuum dry it to complete the grafting modification of the soy protein isolate and obtain modified soy protein.
[0065] 3) Mix the components and their mass ratio:
[0066] Modified soy protein: 99 parts;
[0067] Antioxidant 264: 0.7 parts;
[0068] Antioxidant CA: 0.3 parts;
[0069] 4) dissolving the modified soybean protein in N,N-dimethylformamide according to the ratio, continuously dispersing by ultrasonic for 2 hours until the solution is uniform, and obtaining a spinning solution with a concentration of 30 wt % after keeping the solution at a temperature and degassing;
[0070] 5) The spinning solution was ejected from a 0.15 mm spinneret, cooled in a -5°C air cooler and a 2°C water bath to obtain nascent fibers, and then the nascent fibers were extracted with tetrahydrofuran solvent at 20°C for 40 min, dried at 30°C for 1 h, and then heat-stretched at a heat-stretching temperature of 120°C, a stretching multiple of 30 times, and a heat-setting time of 20 min to obtain modified soybean protein fibers;
[0071] 6) Components and mass ratio:
[0072] Modified soy protein fiber: 95 parts
[0073] Castor oil: 1 part
[0074] Phosphite: 4 parts
[0075] 7) adding the prepared modified soybean protein fiber and castor oil to 60° C. sterile water, keeping warm and softening for 24 hours, and then breaking the softened fiber by 150 kHz ultrasound to obtain ultra-short fibers;
[0076] 8) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 80 kHz for 30 min, settling for 10 min, repeating this process three times to obtain a modified soybean protein fiber web;
[0077] 9) Add phosphite and then vacuum to 5x10 -8 Pa, keep the temperature for 180 min, then return to 45 °C and normal pressure for standby use;
[0078] The fiber web was subjected to hydroentanglement treatment at a water pressure of 30 kPa, with the front side sprayed for 5 minutes and the back side sprayed for 3 minutes, alternating between the front and back sides for 15 times, to obtain a hydroentangled modified soybean protein fiber web;
[0079] 10) The spunlace modified soybean protein fiber web is washed with sterile water, dried, cut and packaged to obtain a modified soybean protein non-woven fabric.
[0080] Example 3
[0081] 1) Disperse soy protein isolate in 6.5 mol / L urea solution under nitrogen atmosphere, stir for 1 h in a 35°C water bath, adjust pH to 8 with sodium hydroxide solution, heat to 80°C, react for 2 h, and activate the soy protein isolate.
[0082] 2) Adjust the grafting reaction temperature to 80°C, add ascorbic acid after the temperature stabilizes, stir for 10 minutes, add ethyl methacrylate as the grafting monomer, and the grafting reaction time is 3 hours. Generate a water-insoluble copolymer product, remove the product, wash it repeatedly, and vacuum dry it to complete the grafting modification of the soy protein isolate and obtain modified soy protein.
[0083] 3) Mix the components and their mass ratio:
[0084] Modified soy protein: 98 parts;
[0085] Antioxidant 1010: 1.4 parts;
[0086] Antioxidant DLTP: 0.6 parts;
[0087] 4) dissolving the modified soy protein isolate in N,N-dimethylformamide according to the ratio, continuously dispersing by ultrasonic for 1 hour until the solution is uniform, and obtaining a spinning solution with a concentration of 15 wt % after heat preservation and static degassing;
[0088] 5) The spinning solution was ejected from a 0.08 mm spinneret, cooled in a 10° C. air cooler and a 5° C. water bath to obtain nascent fibers, and then the nascent fibers were extracted with acetone solvent at 30° C. for 30 min, dried at 50° C. for 12 h, and then heat-stretched and shaped at a heat-stretching temperature of 100° C., a stretching multiple of 10 times, and a heat-setting time of 10 min to obtain modified soybean protein fibers;
[0089] 6) Components and mass ratio:
[0090] Modified soy protein fiber: 92 parts
[0091] Sulfonated oil: 4 parts
[0092] Polyol: 2 parts
[0093] Tall oil: 2 parts
[0094] 7) adding the prepared modified soybean protein fiber, sulfonated oil and castor oil to 60° C. sterile water, keeping warm and softening for 24 hours, and then breaking the softened fiber by 150 kHz ultrasound to obtain ultra-short fibers;
[0095] 8) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 80 kHz for 30 min, settling for 10 min, repeating this process three times to obtain a modified soybean protein fiber web;
[0096] 9) Add polyol and tall oil, and then evacuate to 5x10 -8 Pa, keep warm for 120 min, then return to 45 °C and normal pressure for standby use;
[0097] The fiber web was subjected to hydroentanglement treatment at a water pressure of 30 kPa, with the front side sprayed for 8 minutes and the back side sprayed for 5 minutes, alternating between the front and back sides for 15 times, to obtain a hydroentangled modified soybean protein fiber web;
[0098] 10) The spunlace modified soybean protein fiber web is washed with sterile water, dried, cut and packaged to obtain a modified soybean protein non-woven fabric.
[0099] Example 4
[0100] 1) Disperse soy protein isolate in 8 mol / L urea solution under nitrogen atmosphere, stir for 1 h in a 35°C water bath, adjust pH to 8 with sodium hydroxide solution, heat to 80°C, react for 2 h, and activate the soy protein isolate.
[0101] 2) Adjust the grafting reaction temperature to 80°C, add ammonium cerium sulfate after the temperature stabilizes, stir for 10 minutes, add ethyl methacrylate as the grafting monomer, and the grafting reaction time is 3 hours. Generate a water-insoluble copolymer product, remove the product, wash it repeatedly, and vacuum dry it to complete the grafting modification of the soy protein isolate and obtain modified soy protein.
[0102] 3) Mix the components and their mass ratio:
[0103] Modified soy protein: 65 parts;
[0104] Polyethyl methacrylate: 34 parts
[0105] Antioxidant 1010: 0.7 parts;
[0106] Antioxidant CA: 0.3 parts;
[0107] 4) dissolving the modified soybean protein in acetone according to the ratio, continuously dispersing by ultrasonic for 2 hours until the solution is uniform, and obtaining a spinning solution with a concentration of 10 wt % after keeping the solution warm and degassing;
[0108] 5) The spinning solution was ejected from a 0.1 mm spinneret and cooled in a 20° C. air cooler and a 5° C. water bath to obtain nascent fibers, which were then extracted with an acetone solvent at 25° C. for 60 min and dried at 50° C. for 10 h, and then heat-stretched and shaped at a heat-stretching temperature of 80° C., a stretching multiple of 25 times, and a heat-setting time of 10 min to obtain modified soybean protein fibers;
[0109] 6) Components and mass ratio:
[0110] Modified soy protein fiber: 98 parts
[0111] Birch bark tar: 1 part
[0112] Abietic acid: 1 part
[0113] 7) adding the prepared modified soybean protein fiber and birch bark tar into sterile water at 30°C, keeping warm and softening for 23 hours, and then breaking the softened fiber by 150kHz ultrasound to obtain ultra-short fibers;
[0114] 8) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 100 kHz for 30 minutes, and settling for 15 minutes, repeating this process three times to obtain a modified soybean protein fiber web;
[0115] 9) Add rosin acid and then vacuum to 5x10 -8 Pa, keep warm for 120 min, then return to 45 °C and normal pressure for standby use;
[0116] The fiber web was subjected to hydroentanglement treatment at a water pressure of 50 kPa, with the front side sprayed for 15 minutes and the back side sprayed for 5 minutes, alternating between the front and back sides for 5 times, to obtain a hydroentangled modified soybean protein fiber web;
[0117] 10) The spunlace modified soybean protein fiber web is washed with sterile water, dried, cut and packaged to obtain a modified soybean protein non-woven fabric.
[0118] Example 5
[0119] 1) Disperse soy protein isolate in 5 mol / L urea solution under nitrogen atmosphere, stir in a 40°C water bath for 1 hour, adjust pH to 8 with sodium hydroxide solution, raise temperature to 75°C, react for 2 hours, and activate the soy protein isolate.
[0120] 2) Adjust the grafting reaction temperature to 70°C, add ascorbic acid after the temperature stabilizes, stir for 10 minutes, add ethyl methacrylate as the grafting monomer, and the grafting reaction time is 6 hours. Generate a water-insoluble copolymer product, remove the product, wash it repeatedly, and vacuum dry it to complete the grafting modification of the soy protein isolate and obtain modified soy protein.
[0121] 3) Mix the components and their mass ratio:
[0122] Modified soy protein: 97.5 parts;
[0123] Antioxidant CA: 0.5 parts;
[0124] Antioxidant DLTP: 1 part;
[0125] 4) dissolving the modified soybean protein in the mixture according to the ratio, and continuously dispersing by ultrasonic for 2 hours until the solution is uniform, and obtaining a spinning solution with a concentration of 5 wt % after heat preservation and static degassing;
[0126] 5) The spinning solution was ejected from a 0.6 mm spinneret and passed through an air cooler at 10° C. to obtain nascent fibers; the nascent fibers were then extracted with tetrahydrofuran solvent at 10° C. for 20 min, dried at 30° C. for 24 h, and then heat-stretched and shaped at a heat-stretching temperature of 60° C., a stretching multiple of 5 times, and a heat-setting time of 30 min to obtain modified soybean protein fibers;
[0127] 6) Components and mass ratio:
[0128] Modified soy protein fiber: 97 parts
[0129] Birch bark tar: 1 part
[0130] Abietic acid: 2 parts
[0131] 7) adding birch bark tar to the prepared modified soybean protein fiber in sterile water at 30° C., keeping warm and softening for 15 hours, and then breaking the softened fiber by 130 kHz ultrasound to obtain ultrashort fibers;
[0132] 8) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 100 kHz for 20 minutes, and settling for 25 minutes, repeating this process three times to obtain a modified soybean protein fiber web;
[0133] 9) Add rosin acid and then vacuum to 5x10 -8 Pa, keep the temperature for 130 min, then return to 50 °C and normal pressure for standby use;
[0134] The fiber web was treated with hydroentanglement at a water pressure of 52 kPa, with the front side sprayed for 14 minutes and the back side sprayed for 4 minutes, alternating between the front and back sides for 5 times, to obtain a hydroentangled modified soybean protein fiber web;
[0135] 10) The spunlace modified soybean protein fiber web is washed with sterile water, dried, cut and packaged to obtain a modified soybean protein non-woven fabric.
[0136] The raw materials listed in the present invention, as well as the upper and lower limits and interval values of the raw materials of the present invention, and the upper and lower limits and interval values of the process parameters (such as temperature, time, etc.) can all realize the present invention, and the embodiments are not listed one by one here.
[0137] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.
Claims
1. A method for preparing a modified soybean protein nonwoven fabric, characterized in that: The following steps are involved: 1) Take the following components by mass: 92-98 parts of modified soybean protein fiber, 1-4 parts of softener, and 1-4 parts of stabilizer; Step 1) The modified soybean protein fiber is prepared as follows: 1.1), according to the mass parts of the following components: modified soy protein 92 ~ 98 parts, softener 1 ~ 4 parts, stabilizer 1 ~ 4 parts; In step 1.1), the modified soy protein is prepared as follows: 1) Add soy protein isolate and urea solution into the reactor and heat at 30-50℃ under nitrogen atmosphere. o C water bath, stir for 1-1.5 h, adjust pH to 8-10 with sodium hydroxide, and then raise the temperature to 60-90 o C, react for 1 to 2 h to allow the protein molecules to fully stretch in the solution and open the disulfide bonds; 2) Adjust the water bath temperature to 50-80 o C, after the temperature stabilizes, add the initiator, stir for 10-20 min, slowly drop the reaction grafting monomer, control the drop time to 30-50 min, the stirring speed to 150-200 rpm, and set the grafting time to 2-6 h; 3) Allow the sample solution to settle and filter the precipitate. Wash it with water 3 to 5 times to remove unreacted inorganic salts. After filtering, place it in a vacuum drying oven and evacuate it to 100 to 150 Pa. o C for 12 to 48 h to obtain modified soybean protein; 1.2) Dissolve the mixture in step 1.1) in the solvent according to the ratio, continue ultrasonic dispersion for 1 to 2.5 h until the solution is uniform, and o C, and then the spinning solution with a concentration of 5 to 30 wt% is obtained after static degassing; 1.3) The spinning solution is ejected from the spinneret with an aperture range of 0.06 to 0.15 mm and passed through 10 to 30 o C air cooler to obtain the nascent fiber, after 2 to 10 o C After cooling in a water bath, the initial gel fiber was obtained; 1.4) Place the initial gel fiber in the extractant for extraction for 20 to 60 minutes, and place the extracted initial gel fiber at 40 to 70 o C for 8 to 24 hours to evaporate the excess extractant; 1.5) heat-stretching and shaping the obtained primary fiber to obtain modified soybean protein fiber; 2) The modified soybean protein fiber is heated to 30-60 o C. Add softener into sterile water, keep warm and soften for 12 to 24 hours, and then break the softened fiber by ultrasound to obtain ultra-short fiber; 3) Laying the ultrashort fibers on a fiber web template, ultrasonically oscillating at 80-100 kHz for 10-30 min, settling for 10-30 min, repeating 3-5 times, and obtaining a modified soybean protein fiber web; 4) Add stabilizer and then vacuum to 5x10 -8 Pa, keep warm for 120-180 min, then return to 45-50 o C. Normal pressure standby; 5) The fiber web is spunlaced to obtain a spunlaced modified soybean protein fiber web, and the spunlaced modified soybean protein fiber web is washed with sterile water, dried, cut, and packaged to obtain a modified soybean protein non-woven fabric.
2. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: Step 1) the softening agent is one or more of sulfonated oil, castor oil, birch bark tar and silicone oil; The stabilizer is any one or more of phosphite, rosin acid, polyol and tall oil.
3. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: In step 2), the ultrasonic crushing frequency is 100-150 kHz, and the time is 30-60 min. In step 5), the water pressure is 30-60 kPa during the hydroentanglement treatment, and the front side is sprayed for 5-15 min, and the back side is sprayed for 3-5 min, alternating between the front and back sides for 5-15 times.
4. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: In step 1.1), the softening agent is one or more of sulfonated oil, castor oil, birch bark tar and silicone oil; The stabilizer is any one or more of phosphite, rosin acid, polyol and tall oil.
5. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: In step 1.2), the solvent is one or more of N,N-dimethylformamide, acetone, ether, and tetrahydrofuran, and the ultrasonic dispersion frequency is 30 to 50 kHz; In step 1.4), the extractant is one of acetone and tetrahydrofuran or a combination thereof.
6. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: In step 1.5), the heat stretching is specifically: the heat stretching temperature is 60 to 120 o C, heat stretching and shaping is carried out under the conditions of stretching multiple of 5 to 30 times and heat setting time of 3 to 20 minutes.
7. The method for preparing the modified soybean protein nonwoven fabric according to claim 1, characterized in that: In step 1), the mass ratio of soy protein isolate to urea solution is 1:2 to 1:10, and the concentration of urea solution is 2 to 8 mol / L; In step 2), the initiator is one or a mixture of sodium sulfite, ammonium persulfate, cerium ammonium nitrate, ferrous sulfate, sodium bisulfite, ammonium ferrous sulfate, thiourea, and ascorbic acid; The grafting monomer is one of methyl methacrylate, ethyl methacrylate, butyl methacrylate and hexyl methacrylate, or a mixture of several of them.
8. A modified soybean protein nonwoven fabric prepared according to the preparation method according to any one of claims 1 to 7, characterized in that: The modified soybean protein nonwoven fabric has a Young's modulus of 15-20 GPa and a breaking elongation of 8-12%.
Citation Information
Patent Citations
Modified soybean protein fibres
CN101886297A
Soy protein fibers and preparation method thereof
CN102220650A
Method of photosensitive modification of soybean protein
CN107722195A
Modified soybean isolate protein blasting bead material and preparation method thereof