Non-woven wiping sheet, preparation method and firearm wiping cloth
By adding orange petal fibers to the non-woven fabric and performing hydrotonic fiber opening, combining hydrophilic polyester fibers to form an efficient gun wipe material, the problem that the prior art cannot meet the high mechanical strength and friction requirements of gun wipe are solved. Efficient dirt removal and gun maintenance are achieved.
Patent Information
- Application Number
- CN202211576135.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-09
AI Technical Summary
The existing cleaning wipe materials cannot meet the high mechanical strength and friction requirements when wiping firearms, especially when cleaning the barrel, the shell debris and gunpowder residue cannot be effectively removed.
Add orange petal fibers to the non-woven fabric and open the fibers into microfibers through hydrospinning process. Combining hydrophilic polyester fibers, forming alternately arranged polyamide and polyester fiber structures to improve the mechanical strength of the non-woven wipe sheets , liquid absorption rate and friction force.
Improve the wiping accuracy and friction of the non-woven wipe sheet, effectively remove dirt on the surface and barrel of the gun, reduce fiber breakage and hooking, improve cleaning efficiency, and use the maintenance oil composition to ensure the firearm maintenance. More convenient and efficient.
Smart Images

Figure CN115928319B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonwoven fabrics, and in particular to a nonwoven wiping sheet, a wiping sheet and a firearm wiping cloth. Background Art
[0002] Non-woven sheets have the advantages of not producing fiber dust, being flexible and having low production costs, and are increasingly being used as cleaning and wiping materials. After the gun is used, there are shell fragments, gunpowder residues and other dirt attached to it, which puts forward higher mechanical strength and friction requirements for gun wiping materials, especially barrel wiping materials. Conventional cleaning and wiping materials cannot meet the above requirements. Summary of the invention
[0003] One of the purposes of the present invention is to overcome the defects existing in the prior art and provide a non-woven wiping sheet. Orange peel fibers are added to the non-woven raw material, the orange peel fibers are opened into ultra-fine denier fibers by hydroentanglement, and the ultra-fine denier fibers, unopened orange peel fibers and polyester are entangled by hydroentanglement. The obtained non-woven wiping sheet has good mechanical strength, liquid absorption rate, wiping accuracy and friction.
[0004] In order to achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a non-woven wiping sheet is a spunlace non-woven fabric, the raw material fibers of the spunlace non-woven fabric are mainly composed of hydrophilic polyester fibers and pie fibers; the pie fibers in the non-woven wiping sheet include spunlace opened ultrafine denier fibers and unopened pie fibers, and the alternating pie fiber materials of the pie fibers are polyamide and polyester, respectively. The pie fibers in the non-woven wiping sheet also include pie fiber bundles that are opened but split into ultrafine denier fibers.
[0005] The preferred technical solution is that, by mass percentage, the raw material fibers of the spunlace nonwoven fabric are mainly composed of: 22% to 37% of orange segment fibers and 63% to 78% of hydrophilic polyester fibers. Further, the sum of the mass percentages of orange segment fibers and hydrophilic polyester fibers in the raw material fibers of the spunlace nonwoven fabric is not less than 90%, further, not less than 95%, and further, equal to 100%. Further, the raw material fibers of the spunlace nonwoven fabric are mainly composed of: 28% to 37% of orange segment fibers and 63% to 72% of hydrophilic polyester fibers.
[0006] The preferred technical solution is that, taking the total number of orange-pearl fibers in the 200-fold magnified image of the nonwoven wiping sheet as 100%, the proportion of the hydroentangled ultrafine denier petal fibers in the nonwoven wiping sheet is 65% to 85%; further, the proportion of the hydroentangled ultrafine denier petal fibers is 70% to 80%. The petal fiber bundles are included in the fiber opening.
[0007] The preferred technical solution is that the fiber fineness of the orange segment fiber is 1.7-2.5 dtex; based on the mass of the orange segment fiber as 100%, the mass percentage of the polyester segment fiber in the orange segment fiber is 63%-82%. Further, the mass percentage of the polyester segment fiber is 67%-78%, and further, the mass percentage of the polyester segment fiber is 64%-75%. Further, the fineness of the polyester fiber is 1.5-1.6 dtex. Further, the fineness of a single segment fiber after fiber opening is 0.1-0.15 dtex.
[0008] The second object of the present invention is to provide a method for preparing a nonwoven wiping sheet, comprising the following steps:
[0009] S1: prepare and mix the raw fibers of non-woven fabrics, open and lay the web, and stretch the web;
[0010] S2: The fiber web is conveyed by a rotating drum, and the fiber web is pre-wetted by spunlacing, reinforced by spunlacing, and dried in sequence to obtain a non-woven fabric product;
[0011] The raw material fibers of the non-woven fabric are mainly composed of hydrophilic polyester fibers and orange segment fibers; the materials of the alternately arranged segment fibers of the orange segment fibers are polyamide and polyester respectively.
[0012] The preferred technical solution is that the water spunlace pressure of the reinforced fiber web in S2 is 80-130 MPa, and further, the weight of the fiber web is 50-100 g / m 2 Furthermore, the weight of the fiber web is 60 to 70 g / m 2 .
[0013] The preferred technical solution is that the fiber web obtained by laying in S1 includes straight-laid layers and at least two cross-laid layers stacked sequentially from the front to the back, and the fiber web is reinforced by double-sided spunlace. Furthermore, the front spunlace pressure is 80-90Mpa, and the back spunlace pressure is 85-130Mpa.
[0014] The semi-cross-laid structure composed of straight-laid layers and cross-laid layers is beneficial to improving the longitudinal strength, as well as the uniformity of the fabric's weight, thickness and strength, and reducing the number of abnormal performance points on the fabric.
[0015] The preferred technical solution is that the spunlace needle holes for reinforcing the fiber web include first spunlace needle holes on the front side of the spunlace fiber web and second spunlace needle holes on the back side of the spunlace fiber web, the first spunlace needle holes and the second spunlace needle holes are arranged in rows along the width direction of the fiber web, and the fiber web is spunlace-reinforced by a plurality of rows of first spunlace needle holes and a plurality of rows of second spunlace needle holes, and the spunlace pressure of the spunlace needle holes for reinforcing the fiber web gradually increases along the feeding direction of the fiber web. Further, the number of the first spunlace needle holes is two rows, and further, the number of the second spunlace needle holes is three rows.
[0016] The preferred technical solution is that the distance between the water needle plate for reinforcing the fiber web and the rotating drum is 12-14 mm, the diameter of the water needle holes of the water needle plate is 130-140 μm, and the arrangement density of the water needle holes is 18-20 / cm.
[0017] The second object of the present invention is to provide a firearm wiping cloth, comprising the above-mentioned non-woven wiping sheet, wherein the wiping sheet is impregnated with a curing oil composition;
[0018] The main components of the maintenance oil composition are base oil, film former, rust inhibitor, extrusion additive, antioxidant and dispersant. Further, the kinematic viscosity of the maintenance oil composition is not less than 9.0 mm at 40°C. 2 / s.
[0019] Furthermore, the main components of the maintenance oil composition are, by mass percentage, 83% to 92% of base oil (selected from at least one of poly-α-olefins, mineral oils and ester oils), 5% to 12% of film-forming material (amide-ammonium salt formed by the reaction of octadecylamine and dodecenyl succinic anhydride), and 3% to 5% of rust inhibitor (a composite of 40% by mass of sodium petroleum sulfonate, 40% by mass of dodecenyl succinic acid and 20% by mass of oxidized paraffin).
[0020] The advantages and beneficial effects of the present invention are:
[0021] The raw material fibers of the nonwoven wiping sheet of the present invention include orange segment fibers, and the orange segment fibers are hydroentangled to obtain ultrafine denier fibers. The increase of ultrafine denier fibers within a certain range is conducive to reducing the size of fiber gaps and increasing the number of fiber gaps. The nonwoven fabric has high wiping accuracy and is also conducive to enhancing the overall wicking effect of the nonwoven fabric. The appropriate ratio of orange segment fibers to hydrophilic polyester fibers is conducive to increasing the liquid absorption capacity of the nonwoven fabric.
[0022] The fiber material of the pie fiber is polyamide and polyester. The ultrafine fiber after opening has fiber edges. There is a difference in the fineness of the pie fiber before and after opening. The above two factors are conducive to increasing the friction of the non-woven fabric within a certain range and optimizing the wiping effect.
[0023] The ultra-fine fiber of the orange peel fiber is also conducive to dispersing the fiber force. Compared with the conventional polyester-viscose non-woven fabric for cleaning, the mixed fiber non-woven fabric of orange peel fiber and polyester fiber has better breaking strength;
[0024] The non-woven wiping sheet can effectively wipe the shell debris and gunpowder residue on the surface of the gun and the barrel, especially when used with a cleaning rod to penetrate into the barrel. The wiping sheet will not get hooked on the dirt in the barrel or be torn in the barrel, thereby improving the efficiency of cleaning and wiping the gun. The non-woven wiping sheet impregnated with maintenance oil can evenly apply the maintenance oil to the wiping surface, making gun maintenance more convenient and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a microscope sampling picture of the nonwoven wiping sheet of Example 1;
[0026] Figure 2 This is a photo of the gun barrel after being wiped clean by the gun wipe cloth for the first time; DETAILED DESCRIPTION
[0027] The specific implementation of the present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.
[0028] Fiber composition in nonwoven wipes
[0029] The fibers in the nonwoven fabric are mainly composed of hydrophilic polyester fibers and pie fibers, and the hydrophilic polyester is a polyester fiber that has been hydrophilically finished. The opening of the hydrophilic polyester fiber and the pie fiber affects the liquid absorption capacity of the nonwoven fabric. The number of pie fibers includes but is not limited to 36 petals, 24 petals, 16 petals, and 6 petals. Pie fibers can also be divided into hollow fibers and non-hollow fibers. The more preferred pie fiber in the nonwoven wiping sheet is the hollow pie fiber.
[0030] The selection of pie-shaped fiber, the content of pie-shaped fiber in the raw fiber of nonwoven fabric and the fiber opening ratio of pie-shaped fiber after hydroentanglement will affect the mechanical strength, liquid absorption rate, wiping accuracy and friction of nonwoven wiping sheet.
[0031] Example
[0032] Embodiment 1 Nonwoven wiping sheet material is produced according to the following method:
[0033] S1 fiber configuration: hydrophilic polyester fiber and orange segment fiber are configured respectively;
[0034] Hydrophilic polyester parameters: 1.5dtex;
[0035] Orange segment fiber parameters: The hollow orange segment fiber is composed of 8 parts of polyester (PET) and 8 parts of polyamide (PA) arranged alternately, and the volume ratio of polyester to polyamide in the orange segment fiber is 7:3. The fiber fineness is 17.8±1.2μm / 2.2dtex, and the hollow circle diameter is 4.2±0.8μm.
[0036] S2 prepares the cotton web: configure and mix the fibers according to 30% orange peel and 70% hydrophilic polyester, and introduce the mixed fibers into the production equipment in the following order: automatic weighing and mixing → multiple feeders → conveyor curtain + mixing rollers → opener → cotton storage box → cotton feeding box → carding machine → web laying machine, which first lays one layer of straight web and then two layers of cross-laying web; in the fiber web with three-layer layup structure, the straight-laying layer is located on the front side of the fiber web, and the cross-laying layer is located on the back side of the fiber web;
[0037] S3 spunlace: The fiber web is introduced into the lower drum and upper drum of the spunlace machine. The fiber web passes through the pre-wet spunlace needle holes, two rows of spunlace needle holes on the side of the front side of the fiber web, and three rows of spunlace needle holes on the side of the back side of the fiber web in sequence. The rows of spunlace needle holes are arranged at intervals along the feeding direction of the fiber web;
[0038] The spunlace sequence is: pre-wetting spunlace, spunlace with spunlace needle holes facing the straight-laid layer (front spunlace), spunlace with spunlace needle holes facing the cross-laid layer (back spunlace), and the spunlace pressures of each spunlace step are:
[0039] Pre-wetted spunlace: 35MPa;
[0040] Frontal water jetting of two rows of needle holes: 50MPa, 8MPa;
[0041] Three types of reverse spurting needle holes: 85MPa, 115MPa, 120MPa;
[0042] The process parameters of the spunlace needle board are as follows: the distance between the spunlace needle board for reinforcing the fiber web and the rotating drum is 13 mm, the diameter of the spunlace needle holes of the spunlace needle board is 135 μm, and the arrangement density of the spunlace needle holes is 20 / cm.
[0043] S4 reinforced fiber web export: the exported fiber web is dried at 120°C, and the fiber web feeding speed is 50m / min to obtain non-woven fabric.
[0044] Example 2
[0045] Example 2 is based on Example 1, and the fiber configuration ratio is changed. The fiber ratio of Example 2 is 70% orange peel fiber and 30% hydrophilic polyester fiber. The models of the orange peel fiber and hydrophilic polyester fiber used are the same as those in Example 1.
[0046] Comparative Example 1
[0047] Comparative Example 1 is based on Example 1, but the fiber configuration ratio is changed. The fiber ratio of Comparative Example 1 is 65% polyester fiber, 30% viscose fiber, and 5% ES fiber. The polyester fiber is a conventional polyester fiber instead of the hydrophilic polyester fiber in Example 1. The fiber fineness of the polyester fiber, viscose fiber, and ES fiber is all 1.56 dtex.
[0048] The following performance tests were performed on the samples of Examples 1, 2 and Comparative Example 1:
[0049] 1. Test the liquid absorption of non-woven wiping sheet samples according to GB / T 24218.6-2010;
[0050] 2. Test the breaking strength of non-woven wiping sheet samples according to GB / T 24218.3-2010;
[0051] 3. Test the friction coefficient of non-woven wiping sheet samples according to GB / T 10006-2021;
[0052] 4. The non-woven wiping sheet is loaded with 200% liquid, and the liquid is a curing oil composition;
[0053] The composition of the maintenance oil composition is as follows: the main components of the maintenance oil composition are: 88% of base oil mineral oil, 7% of film-forming material (amide-ammonium salt formed by the reaction of octadecylamine and dodecenyl succinic anhydride), 5% of rust inhibitor (composite of 40% by mass of sodium petroleum sulfonate, 40% by mass of dodecenyl succinic acid and 20% by mass of oxidized paraffin);
[0054] Gun barrel wiping method: Cut the dry non-woven wiping sheet into 1.5*10cm strips, insert the strip wiping sheet into the cleaning rod, and the cleaning rod carries the wiping sheet into the gun barrel; wipe once and then wipe again, and visually compare the amount of gun barrel stains remaining on the second wiping sheet.
[0055] like Figure 1 As shown, in the 200-fold microscope magnification image, the fiber with the finest fiber fineness is the ultrafine denier fiber obtained by opening the orange peel fiber, the fiber with the coarsest fiber fineness is the orange peel fiber (with obvious orange peel structure), the fiber with a smooth surface and a medium fiber fineness is the hydrophilic polyester fiber, and the petal fiber bundle has an obvious petal structure.
[0056] The test results of the non-woven wiping sheets of Examples 1, 2 and Comparative Example 1 are shown in the following table:
[0057]
[0058]
[0059] *Split pie fiber opening ratio: the percentage of split pie fibers to the total number of pie fibers in the microscope magnified image. The number of pie fibers sampled in the embodiment is 1000.
[0060] Figure 2 This is a photo of one wiping; visual inspection results of gun barrel wiping with non-woven wiping sheet: compared with Example 2 and Comparative Example 1, the sample of Example 1 has less secondary wiping residue in the gun barrel.
[0061] In the above table, Example 1 and Comparative Example 1 form a comparison of the raw material fibers of the non-woven wiping sheet. The hydrophilic fiber content in Comparative Document 1 is higher, and the ultra-fine denier fiber is conducive to forming a wicking effect. The water absorption multiple of Example 1 is higher than that of Comparative Example 1;
[0062] The breaking strength, dynamic friction and static friction of Example 1 are significantly better than those of Comparative Example 1. The non-woven wiping sheet Examples 1-2 can be stably inserted into the cleaning rod and separated from the gun barrel without hooking in the gun barrel, fiber shedding and retention in the gun barrel, and non-woven fabric tearing in the gun barrel;
[0063] Example 1 and Example 2 form a comparison of the content of pie fiber and hydrophilic polyester fiber. On the basis of the fiber content in Example 1, the pie fiber is further increased while the hydrophilic polyester fiber is reduced. The water absorption multiple is not increased but decreased, and the static friction and dynamic friction coefficients are significantly reduced. The reason is that the pie fiber content is too high, and the spunlace process cannot open the fibers better, resulting in a small difference in fiber fineness on the surface of the non-woven fabric.
[0064] Example 3
[0065] Based on the same production equipment as in Example 1 (the distance between the spunlace needle plate and the drum, the spunlace needle hole diameter, the spunlace needle hole density, and the web feeding speed are the same), the spunlace pressure of the non-woven wiping sheet production process in Example 3 is as follows:
[0066] Pre-wetted spunlace: 35MPa;
[0067] Frontal water jetting of two rows of needle holes: 60MPa, 85MPa;
[0068] The reverse side water jet of three types of row needle holes: 90MPa, 120MPa, 133MPa.
[0069] Example 4
[0070] Based on the same production equipment as in Example 1 (the distance between the spunlace needle plate and the drum, the spunlace needle hole diameter, and the spunlace needle hole density are the same), the spunlace pressure of the non-woven wiping sheet production process in Examples 3 and 4 is as follows:
[0071] Pre-wetted spunlace: 35MPa;
[0072] Frontal water jetting of two rows of needle holes: 50MPa, 75MPa;
[0073] Three types of reverse spurting needle holes: 85MPa, 105MPa, 115MPa;
[0074] The fiber opening ratio and breaking strength of Example 1, Example 3 and Example 4 are shown in the following table:
[0075]
[0076] The second wiping residues in Examples 3 and 4 are more than that in Example 1.
[0077] In the magnified image of the nonwoven wiping sheet sample of Example 3, some of the ultrafine fibers are broken. The reason is that the water spunlace pressure during the reinforcement of the web is too large, which breaks some of the ultrafine fibers, which is manifested as a decrease in the horizontal and vertical breaking strength of the nonwoven wiping sheet; the fiber opening rate of the orange segment fiber is increased, the proportion of ultrafine fibers on the surface of the nonwoven wiping material is higher, and the static friction coefficient and dynamic friction coefficient are lower than those of Example 1.
[0078] According to the water spunlace pressure of the reinforced web in Example 4, the opening ratio of the orange peel fibers in the non-woven wiping sheet sample is low. Although the breaking strength is higher than that in Example 1, the total number of fiber edges after opening is small. The difference in fineness between the orange peel fibers and the hydrophilic polyester fibers on the surface of the non-woven wiping sheet sample is not obvious, so the static friction coefficient and the dynamic friction coefficient are reduced.
[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a nonwoven wiping sheet, characterized in that: The following steps are involved: S1: prepare and mix the raw fibers of non-woven fabrics, open and lay the web, and stretch the web; S2: The fiber web is conveyed by a rotating drum, and the fiber web is pre-wetted by spunlacing, reinforced by spunlacing, and dried in sequence to obtain a non-woven fabric product; The non-woven wiping sheet is a spunlace non-woven fabric, and the raw material fibers of the spunlace non-woven fabric are mainly composed of hydrophilic polyester fibers and pie fibers; the pie fibers in the non-woven wiping sheet include spunlace-opened ultrafine denier fibers and unopened pie fibers, and the alternatingly arranged pie fibers are made of polyamide and polyester respectively; The raw material fibers of the spunlace nonwoven fabric are mainly composed of 22% to 37% orange peel fibers and 63% to 78% hydrophilic polyester fibers by mass percentage; taking the total number of orange peel fibers in the 200-fold magnified image of the nonwoven wiping sheet as 100%, the proportion of the spunlace-opened ultrafine denier peel fibers in the nonwoven wiping sheet is 65% to 85%; the fiber fineness of the orange peel fibers is 1.7 to 2.5 dtex; taking the mass of the orange peel fibers as 100%, the mass percentage of the polyester peel fibers in the orange peel fibers is 63% to 82%; The fiber web obtained by laying the web in S1 includes straight-laid layers and at least two cross-laid layers stacked in sequence from the front side to the back side, and the fiber web is reinforced by double-sided spunlace; The water spunlace pressure of the reinforced fiber web in S2 is 80-130 MPa, and the gram weight of the fiber web is 50-100 g / m2.
2. The method for preparing the nonwoven wiping sheet according to claim 1, characterized in that: The spunlace needle holes for reinforcing the fiber web include first spunlace needle holes on the front side of the spunlace fiber web and second spunlace needle holes on the back side of the spunlace fiber web. The first spunlace needle holes and the second spunlace needle holes are arranged in rows along the width direction of the fiber web. The fiber web is spunlace-reinforced by spunlace needle holes in several rows and several rows of second spunlace needle holes. The spunlace pressure of the spunlace needle holes for reinforcing the fiber web gradually increases along the feeding direction of the fiber web.
3. The method for preparing the nonwoven wiping sheet according to claim 1, characterized in that: The distance between the water needle plate for reinforcing the fiber web and the rotating drum is 12-14 mm, the diameter of the water needle holes of the water needle plate is 130-140 μm, and the density of the water needle holes is 18-20 per cm.