A kind of disk-shaped tantalum powder and preparation method thereof
By spheroidizing and spraying the irregular tantalum powder, the flake-shaped tantalum powder is prepared, which solves the problems of irregular tantalum powder particle shape and low production efficiency, and achieves uniform charge distribution and improved voltage resistance. tantalum capacitors with high specific capacitance and high reliability.
Patent Information
- Application Number
- CN202211685827.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-27
AI Technical Summary
In the existing tantalum powder manufacturing process, the tantalum powder has irregular grain shape, high impurity content, and difficult to adjust the diameter and thickness ratio, resulting in uneven charge distribution, easy tip discharge, and low production efficiency, making it impossible to achieve high specific capacity and voltage resistance. Synchronous improvement.
After the irregular tantalum powder is processed through the screen, it is subjected to inductively coupled plasma torch spheroidization, and then annealed in vacuum or protective gas. Finally, it is mixed with the injection system and the high-speed jet to impact the rigid substrate to form a circular tantalum powder. , achieve regular particle shape, low impurity content, and adjustable diameter and thickness ratio.
The prepared flake-shaped tantalum powder has smooth edges, uniform charge distribution, avoiding tip discharge, minimizing specific surface area loss and improving voltage resistance, and safe and sustainable process, improving production efficiency.
Smart Images

Figure CN115945683B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tantalum powder preparation, and in particular to a disc-shaped tantalum powder and a preparation method thereof. Background Art
[0002] Tantalum powder specially used to make tantalum capacitors is called capacitor-grade tantalum powder. Tantalum capacitors are widely used not only in military communications, aerospace and other fields, but also in industrial automation, film and television equipment, personal computers, mobile communications and other fields due to their high specific capacitance, good stability, wide operating temperature range, moisture resistance and shock resistance, high reliability, and easy miniaturization and chip-type.
[0003] According to the different particle shapes and agglomeration states of tantalum powder, it can be divided into high-voltage tantalum powder, medium-voltage tantalum powder, and low-voltage high-specific capacitance tantalum powder. Cabot Corporation of the United States first introduced flaky medium-voltage tantalum powder to the market. Compared with ordinary tantalum powder, flaky tantalum powder has larger particle size, simpler particle shape, better sintering resistance, high voltage resistance, and high reliability. While ensuring the withstand voltage characteristics of tantalum powder, the capacitance reaches an ideal level, which is particularly suitable for making medium-voltage solid tantalum electrolytic capacitors with high reliability requirements of 20V to 63V. The current manufacturing process of flaky tantalum powder is to ball-mill irregular tantalum powder (such as metal Na reduced tantalum powder or EB tantalum powder obtained by hydrogenation and dehydrogenation of electron beam smelting tantalum ingots) to make it flat, and then undergo oxygen reduction and thermal agglomeration treatment to prepare a tantalum powder with primary particles in the form of flakes.
[0004] However, with the continuous improvement of the specific volume of tantalum powder, problems in raw materials and film-making process have gradually become prominent, restricting the continuous development of flaky tantalum powder towards higher specific volume. From the perspective of raw materials, whether it is the reduced tantalum powder with a loose porous structure or the hydrogenated dehydrogenated EB tantalum powder with a polygonal structure, they are all irregular in shape. After ball milling, the shape of this raw material tantalum powder is also irregular flake, and the edge of the tantalum flake is broken to present an irregular sawtooth shape. The flaky tantalum powder with this shape has uneven charge distribution after charging, is prone to tip discharge, and cannot minimize the loss of specific surface area during the high-voltage formation process. From the perspective of film-making process, since the performance of flaky tantalum powder is determined by its diameter-to-thickness ratio, the thinner and smaller the flake, the larger the specific surface area, and the higher the corresponding specific volume. In order to obtain thinner and finer flakes, the method of extending the ball milling time is usually adopted. However, the particle size of tantalum powder does not decrease infinitely with the extension of ball milling time, but there will be a reverse crushing phenomenon of ultrafine powder agglomeration and overall particle size increase. This kind of agglomerated submicron tantalum powder is not only easy to heat up and cause fire, but also easy to be broken down during the pressurization process, and its pressure resistance and stability are reduced. Moreover, the content of metals such as Fe, Ni, Cr and non-metallic impurities such as O and N will be greatly increased when the tantalum powder is ground by a ball mill for a long time. The large-scale production of medium-pressure tantalum powder and the shortcomings of the ball milling process such as high labor intensity and inability to produce continuously seriously restrict the improvement of production efficiency. Therefore, there is currently a lack of a preparation process for a tantalum powder with simple and regular particle shape, low impurity content, and adjustable diameter-to-thickness ratio. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a flaky tantalum powder and a preparation method thereof. The flaky tantalum powder prepared by the preparation method has regular particle shape, low impurity content, and adjustable diameter-to-thickness ratio. After anode charging, the charge distribution is uniform, which can effectively avoid tip discharge and achieve simultaneous improvement in voltage resistance and specific capacitance.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0007] In one aspect, the present invention provides a method for preparing a tantalum flake powder, comprising the following steps:
[0008] Using irregular tantalum powder as raw material, sieving it through a sieve to obtain irregular tantalum powder with a particle size that meets the requirements;
[0009] The irregular tantalum powder with the required particle size is placed in an inductively coupled plasma torch for spheroidization treatment to obtain spherical tantalum powder with regular shape;
[0010] The spherical tantalum powder with regular shape is annealed in a vacuum or protective gas, and after the annealing is completed, the spherical tantalum powder is cooled to room temperature to obtain cooled spherical tantalum powder;
[0011] The cooled spherical tantalum powder is fed into the injection system and mixed with the high-speed jet of the injection system to form a two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it hits the rigid substrate of the injection system and falls from the surface of the rigid substrate to obtain tantalum powder in the form of discs.
[0012] In one embodiment, in the step of using irregular tantalum powder as raw material and sieving it to obtain irregular tantalum powder with a particle size that meets the requirements, the particle size range of the irregular tantalum powder with a particle size that meets the requirements is 5 to 50 microns.
[0013] Furthermore, the irregular tantalum powder is obtained by reducing tantalum powder and melting it into an ingot by electron beam, followed by hydrogenation, crushing and dehydrogenation treatment;
[0014] And\or, the irregular tantalum powder is obtained by reducing tantalum powder through atomization granulation or high-temperature granulation.
[0015] In one embodiment, in the step of placing irregular tantalum powder into an inductively coupled plasma torch for spheroidization to obtain spherical tantalum powder with regular morphology, the process parameters of the inductively coupled plasma torch are set as follows:
[0016]
[0017] In one embodiment, the spherical tantalum powder with regular morphology is annealed in a vacuum or protective gas, and then cooled to room temperature to obtain the cooled spherical tantalum powder. The protective gas is a plurality of or one inert gas, and the annealing temperature is 900°C to 1400°C. The temperature is increased to the temperature at a rate of 10°C / min to 20°C / min, and after reaching the temperature, the treatment is performed for 30 to 90 minutes.
[0018] In one embodiment, the cooled spherical tantalum powder is fed into the injection system and mixed with the high-speed jet of the injection system to form a two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it hits the rigid substrate of the injection system and falls from the surface of the rigid substrate to obtain tantalum flake powder. In the step, the high-speed jet is a high-speed jet generated by the fluid entering the injection system.
[0019] Furthermore, the fluid includes gas or liquid, the gas includes at least one of nitrogen, argon, and compressed air, and the liquid includes at least one of distilled water and ethanol.
[0020] In one embodiment, the cooled spherical tantalum powder is fed into the injection system and mixed with the high-speed jet of the injection system to form a two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it hits the rigid substrate of the injection system and falls from the surface of the rigid substrate to obtain tantalum flake powder. In the step, the injection speed of the two-phase flow after acceleration is 50m / s to 650m / s, and the impact angle is 30° to 90°.
[0021] On the other hand, according to an embodiment of the present invention, there is also provided a disc-shaped tantalum powder, comprising:
[0022] The tantalum flake powder is prepared by the above-mentioned preparation method.
[0023] In one embodiment, the shape of the disc-shaped tantalum powder is a perfect circle or an ellipse;
[0024] The major-minor axis ratio of the flake-shaped tantalum powder is 1:1 to 4:1;
[0025] The diameter-to-thickness ratio of the flake-shaped tantalum powder is 1-20.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The tantalum powder prepared by the preparation method of the present invention is in the shape of a disc, with smooth and regular edge morphology, uniform charge distribution after charging, no tip discharge occurs, and the specific surface area loss can be minimized during the charging process.
[0028] 2. The present invention can flexibly adjust the major-minor axis ratio and the diameter-thickness ratio of the flake-shaped tantalum powder by changing the injection speed of the two-phase flow and the impact angle between the two-phase flow and the rigid substrate, and can achieve a wide range of adjustment of the specific volume and pressure resistance performance.
[0029] 3. The present invention changes the technical route of the traditional film-making method through long-term ball milling to achieve film-making. The one-time forming of tantalum powder in the form of discs is achieved through high-speed collision between spherical tantalum powder and a rigid substrate, thus avoiding the defects of reverse crushing, over-crushing, powder heating and increased impurity content of tantalum powder caused by long-term ball milling.
[0030] 4. The present invention uses a high-speed jet to mix with spherical tantalum powder to form a two-phase flow to impact a rigid substrate to obtain a disc-shaped tantalum powder. The high-speed jet accelerates the spherical tantalum powder and can take away the heat generated during the impact deformation process, avoiding the oxidation and spontaneous combustion of the tantalum powder and production interruption caused by heat accumulation and temperature rise, making the process safer, realizing continuous production, and greatly improving the powder making efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a flow chart of the method for preparing tantalum flake powder.
[0032] Figure 2 This is a scanning electron microscope image of Example 1 of the present invention.
[0033] Figure 3 This is a scanning electron microscope image of Example 2 of the present invention. DETAILED DESCRIPTION
[0034] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0035] In one aspect, the present invention provides a method for preparing tantalum powder in the form of a disk, such as Figure 1 As shown, the following steps are included:
[0036] Step 1: using irregular tantalum powder as raw material, sieving it through a sieve to obtain irregular tantalum powder with a particle size that meets the requirements;
[0037] Step 2: placing irregular tantalum powder with a particle size that meets the requirements into an inductively coupled plasma torch for spheroidization treatment to obtain spherical tantalum powder with a regular shape;
[0038] Step 3, annealing the spherical tantalum powder with regular shape in vacuum or protective gas, and cooling it to room temperature after the annealing to obtain cooled spherical tantalum powder;
[0039] Step 4: The cooled spherical tantalum powder is fed into the injection system and mixed with the high-speed jet of the injection system to form a two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it hits the rigid substrate of the injection system and falls from the surface of the rigid substrate to obtain tantalum powder in the form of discs.
[0040] Furthermore, in step 1, the irregular tantalum powder having the required particle size has a particle size range of 5 to 50 microns, preferably 10 to 30 microns.
[0041] Furthermore, the irregular tantalum powder is obtained by reducing tantalum powder and melting it into an ingot by electron beam, followed by hydrogenation, crushing and dehydrogenation treatment;
[0042] And\or, the irregular tantalum powder is obtained by reducing tantalum powder through atomization granulation or high-temperature granulation.
[0043] Furthermore, in step 2, the process parameters of the inductively coupled plasma torch are set:
[0044]
[0045] Furthermore, in step three, the protective gas is a plurality of or one inert gas, the temperature of the annealing treatment is 900°C to 1400°C, and the temperature is increased to the temperature at a rate of 10°C / min to 20°C / min. After reaching the temperature, the treatment time is 30 to 90 minutes, wherein the preferred protective gas is argon, and the treatment time is 60 to 90 minutes.
[0046] Furthermore, in step four, the high-speed jet is a high-speed jet generated by the fluid entering the injection system.
[0047] Furthermore, the fluid includes gas or liquid, the gas includes at least one of nitrogen, argon, and compressed air, and the liquid includes at least one of distilled water and ethanol, and nitrogen is most preferred.
[0048] Furthermore, in step 4, the injection speed of the two-phase flow after acceleration is 50 m / s to 650 m / s, and the impact angle is 30° to 90°.
[0049] On the other hand, according to an embodiment of the present invention, there is also provided a disc-shaped tantalum powder, comprising:
[0050] The tantalum flake powder is prepared by the above-mentioned preparation method.
[0051] Furthermore, the shape of the disc-shaped tantalum powder is a perfect circle or an ellipse;
[0052] The major-minor axis ratio of the flake-shaped tantalum powder is 1:1 to 4:1;
[0053] The diameter-to-thickness ratio of the flake-shaped tantalum powder is 1-20.
[0054] The tantalum powder prepared by the preparation method of the present invention is in the shape of a disc, with a smooth and regular edge shape, uniform charge distribution after charging, no tip discharge, and the specific surface area loss can be minimized during the charging process. By changing the injection speed of the two-phase flow and the impact angle between the two-phase flow and the rigid substrate, the major-minor axis ratio and the diameter-thickness ratio of the disc-shaped tantalum powder can be flexibly adjusted, and a wide range of specific volume and pressure resistance can be adjusted. The technical route of the traditional film-making method to achieve film-making through long-term ball milling is changed, and the one-time forming of the disc-shaped tantalum powder is achieved by the high-speed impact of the spherical tantalum powder and the rigid substrate, thereby avoiding the defects of reverse crushing, over-crushing, powder heating, and increased impurity content of the tantalum powder caused by long-term ball milling. After mixing with the spherical tantalum powder by high-speed jet, a two-phase flow is formed to impact the rigid substrate to obtain a disc-shaped tantalum powder. While the high-speed jet accelerates the spherical tantalum powder, it can take away the heat generated during the impact deformation process, avoiding the oxidation and spontaneous combustion of the tantalum powder and the interruption of production caused by the increase in heat accumulation and temperature, making the process safer, realizing continuous production, and greatly improving the powder making efficiency.
[0055] The present invention has been tested for many times, and some test results are now cited as references to further describe the invention in detail, and the following is a detailed description in conjunction with specific embodiments.
[0056] Example 1
[0057] The steps for preparing tantalum powder in the form of a disc with a particle size of 20 to 30 microns, a diameter-to-thickness ratio of 10, and a major-minor axis ratio of 1:1 are as follows:
[0058] Step 1: using irregular shaped granulated tantalum powder obtained by high temperature granulation of reduced tantalum powder as raw material, screening the tantalum powder to collect irregular shaped tantalum powder with a particle size range of 10 to 15 microns;
[0059] Step 2: Place the irregular tantalum powder with the required particle size into an inductively coupled plasma torch for spheroidization treatment, and set the process parameters of the inductively coupled plasma torch as follows:
[0060]
[0061]
[0062] After the treatment, spherical tantalum powder with regular shape is obtained;
[0063] Step 3, annealing the spherical tantalum powder with regular shape in argon gas at a temperature of 1100° C., heating to the annealing temperature at a rate of 15° C. / min, and after reaching 1100° C., heat preservation for 60 minutes, and then cooling to room temperature to obtain cooled spherical tantalum powder;
[0064] Step 4: Send distilled water at 70°C and 5MPa into the injection system to generate a high-speed jet, send the cooled spherical tantalum powder into the injection system, and mix with the high-speed jet of the injection system to form a solid-liquid two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it is accelerated to a jet speed of 160-180m / s and hits the rigid substrate of the injection system at 90°. The spherical tantalum powder undergoes plastic deformation and then falls from the surface of the rigid substrate to obtain a flaky tantalum powder with a particle size of 20-30μm, a diameter-to-thickness ratio of 10, and a major-minor axis ratio of 1:1, such as Figure 2 shown.
[0065] Example 2
[0066] The steps for preparing tantalum powder in the form of a disc with a particle size of 35 to 50 μm, an aspect ratio of 5, and a major-minor axis ratio of 2:1 are as follows:
[0067] Step 1, using the irregularly shaped crushed tantalum powder obtained by electron beam melting into ingots and then hydrogenating, crushing and dehydrogenating the reduced tantalum powder as raw material, screening the irregularly shaped tantalum powder with a particle size range of 20 to 30 microns;
[0068] Step 2: Place the irregular tantalum powder with the required particle size into an inductively coupled plasma torch for spheroidization treatment, and set the process parameters of the inductively coupled plasma torch as follows:
[0069]
[0070] After the treatment, spherical tantalum powder with regular shape is obtained;
[0071] Step 3, annealing the spherical tantalum powder with regular shape in argon gas at a temperature of 1150° C., heating to the annealing temperature at a rate of 20° C. / min, and after reaching 1150° C., heat preservation for 75 minutes, and then cooling to room temperature to obtain cooled spherical tantalum powder;
[0072] Step 4: Send compressed nitrogen at 120°C and 12MPa into the injection system to generate a high-speed jet, send the cooled spherical tantalum powder into the injection system, and mix with the high-speed jet of the injection system to form a gas-liquid two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it is accelerated to a jet speed of 100-120m / s and hits the rigid substrate of the injection system at 30°. The spherical tantalum powder undergoes plastic deformation and then falls from the surface of the rigid substrate to obtain a flake-shaped tantalum powder with a particle size of 35-50μm, a diameter-to-thickness ratio of 5, and a major-minor axis ratio of 21:1, as shown in FIG. Figure 3 shown.
Claims
1. A method for preparing a tantalum flake powder for a capacitor, characterized in that: The steps include: Using irregular tantalum powder as raw material, sieving, to obtain irregular tantalum powder with a particle size range of 5~50 microns; Irregular tantalum powder with a particle size range of 5 to 50 microns is placed in an inductively coupled plasma torch for spheroidization to obtain spherical tantalum powder with regular morphology; The spherical tantalum powder with regular shape is annealed in a vacuum or protective gas, and after the annealing is completed, the spherical tantalum powder is cooled to room temperature to obtain cooled spherical tantalum powder; The cooled spherical tantalum powder is sent into the injection system and mixed with the high-speed jet of the injection system to form a two-phase flow. After the two-phase flow is accelerated by the nozzle of the injection system, it hits the rigid substrate of the injection system at a speed of 50m / s~650m / s, and the impact angle is 30°~90°. The spherical tantalum powder is deformed by the impact and falls from the surface of the rigid substrate, and a round or elliptical shape, a major-minor axis ratio of 1:1~4:1, a diameter-thickness ratio of 1~20, and a smooth and regular edge morphology of the round tantalum powder is obtained; The high-speed jet is a high-speed jet generated by a fluid entering a spray system, and the fluid is distilled water at 70° C. and 5 MPa or compressed nitrogen at 120° C. and 12 MPa.
2. The method for preparing a flaky tantalum powder for capacitors according to claim 1, characterized in that: The irregular tantalum powder is obtained by reducing tantalum powder and melting it into an ingot through electron beam, followed by hydrogenation, crushing and dehydrogenation treatment; And\or, the irregular tantalum powder is obtained by atomizing and granulating reduced tantalum powder.
3. The method for preparing a flaky tantalum powder for capacitors according to claim 1, characterized in that: In the step of placing irregular tantalum powder into an inductively coupled plasma torch for spheroidization treatment to obtain spherical tantalum powder with regular morphology, the process parameters of the inductively coupled plasma torch are set as follows: Power 30kW~100kW Working gas flow 10slpm~50slpm argon Side gas flow 30slpm~150slpm argon, 5~20 slpm hydrogen System pressure 40kPa~98kPa Tantalum powder feeding rate is 20g / min~100g / min.
4. The method for preparing a flaky tantalum powder for capacitors according to claim 1, characterized in that: In the step of annealing the spherical tantalum powder with regular morphology in a vacuum or protective gas, and cooling it to room temperature after the treatment to obtain the cooled spherical tantalum powder, the protective gas is a plurality of or one inert gas, the annealing temperature is 900°C to 1400°C, and the temperature is increased to the temperature at a rate of 10°C / min to 20°C / min. After reaching the temperature, the treatment time is 30 to 90 minutes.
5. A tantalum powder in the form of discs for capacitors, prepared by the method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Preparation method for flaky powder
CN105537600A
Preparation method for wave absorbing material with high magnetic conductivity
CN107507689A
Low-oxygen spherical tantalum powder and preparation method thereof
CN110947976A
Production method of high-pressure-resistant flaky tantalum powder
CN112620636A
Method and an Apparatus of Plasma Processing of Tantalum Particles
US20080118391A1