A method for synthesizing single-phase strontium yttrium oxide coating material by low-temperature solid phase method

The low-temperature solid-state method using isopropanol ball milling media and low-temperature heat treatment to synthesize single-phase strontium yttrium solves the problems of high energy consumption and impurity phases in high-temperature synthesis, and realizes the preparation of low-cost, high-purity strontium yttrium.

CN115947366BActive Publication Date: 2024-11-22CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211209093.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-22
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The traditional solid-state synthesis of strontium yttrium oxide requires high-temperature phase formation, resulting in high energy consumption and the product often contains yttrium trioxide impurities, affecting purity and quality.

Method used

Single-phase strontium yttrium was synthesized via a low-temperature solid-state method using isopropanol as the ball milling medium and combined with low-temperature heat treatment. The specific steps included mixing strontium salt and yttrium salt, ball milling, drying, and then heat treatment at 950°C.

Benefits of technology

The synthesis temperature was lowered to 950℃, which reduced energy consumption, avoided yttrium trioxide impurity phase, improved product purity and quality, and provided a low-cost route for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947366B_ABST
    Figure CN115947366B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for synthesizing a single-phase strontium yttrium coating material by a low-temperature solid-phase method. The method for preparing a single-phase strontium yttrium by low-temperature sintering is as follows: first, a divalent strontium salt and a trivalent yttrium salt in a stoichiometric ratio are mixed; then, isopropanol solvent is added to the mixture as a ball milling medium for ball milling; finally, the mixed slurry obtained above is dried; and a heat treatment at not less than 950°C for 2 to 20 hours is performed to obtain a single-phase SrY2O4. The present invention obtains a single-phase strontium yttrium at a relatively low phase formation temperature, has simple process conditions, is easy to control, greatly reduces energy consumption, and saves production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic material preparation, in particular to a method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method. Background Art

[0002] Strontium yttrium (SrY2O4) belongs to the orthorhombic system, space group pnam (62), in which strontium (Sr) is VIII-coordinated and yttrium (Y) is VI-coordinated. The traditional application of strontium yttrium is mainly concentrated in the field of optical materials. However, the structure of strontium yttrium is stable to 2215℃ without phase change, with large thermal expansion coefficient and excellent mechanical properties. It has great potential as an excellent candidate thermal barrier coating ceramic layer material that can replace traditional YSZ thermal barrier coating materials. At the same time, strontium yttrium yttrium materials also have broad application prospects in luminescent materials. When synthesizing strontium yttrium by traditional solid phase method, a higher phase formation temperature (about 1350℃) is generally required, and the synthesized strontium yttrium yttrium usually contains a small amount of yttrium trioxide (Y2O3) impurity phase. Summary of the invention

[0003] The purpose of the present invention is to provide a low-temperature solid-phase method for synthesizing a single-phase strontium yttrium oxide coating material.

[0004] The invention discloses a low-temperature solid-phase method for synthesizing a single-phase strontium yttrium yttrium coating material, wherein the strontium yttrium yttrium is composed of a single phase of SrY2O4.

[0005] A low-temperature solid-phase method for synthesizing a single-phase strontium yttrium oxide coating material of the present invention comprises the following steps:

[0006] (1) mixing strontium salt and yttrium salt in a molar ratio of Sr:Y of 1:2;

[0007] (2) adding isopropanol to the mixture obtained in step (1) and performing high energy ball milling;

[0008] (3) drying the slurry obtained in step (2);

[0009] (4) The powder obtained in step (3) is heat treated at a temperature not lower than 950° C. for 2 to 20 h to obtain a single-phase SrY2O4 powder.

[0010] Furthermore, the strontium salt in step (1) is any one of strontium carbonate, strontium oxalate, strontium nitrate, strontium chloride, strontium acetate or strontium sulfate.

[0011] Furthermore, the yttrium salt in step (1) is any one of yttrium oxide, yttrium nitrate, yttrium chloride, yttrium sulfate or yttrium acetate.

[0012] Furthermore, the ball milling parameters in step (2) are: rotation speed 2000-5000 rpm, zirconia ball mill and ball mill, and ball milling time 5-20 hours.

[0013] Step (3) drying the slurry obtained in step (2) at a temperature of 80 to 105° C. for 10 to 24 hours.

[0014] The beneficial effects of the present invention are:

[0015] (1) The present invention uses isopropanol as a ball milling medium to process powder slurry to prepare strontium yttrium yttrium. The lowest heat treatment phase temperature is 950°C, which can greatly reduce energy consumption and production costs.

[0016] (2) The present invention uses isopropanol as a ball milling medium to treat the powder slurry. The strontium yttrium yttrium prepared by heat treatment at 950°C has a single-phase structure and does not contain yttrium trioxide impurity phase, thereby improving the synthesis purity of industrial strontium yttrium yttrium, which is beneficial to improving product quality.

[0017] (3) The process of the present invention is simple and easy to implement, isopropyl alcohol is cheap and easily available, and has low energy consumption, which provides a new idea for the industrial production of single-phase strontium yttrium oxide prepared by low-temperature sintering. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The X-ray diffraction pattern (XRD) of the strontium yttrium powder synthesized by the present invention is kept at 950°C for 5 hours. The powder obtained by retrieval is strontium yttrium yttrium SrY2O4 single-phase composition JCPDS (PDF 74-0264).

[0019] Figure 2 The X-ray diffraction pattern (XRD) of the strontium yttrium powder synthesized by the present invention is kept at 950°C for 10 hours. The powder obtained by retrieval is strontium yttrium yttrium SrY2O4 single-phase composition JCPDS (PDF 74-0264).

[0020] Figure 3 The present invention discloses an X-ray diffraction spectrum of a powder containing a heterophase Y2O3 synthesized by ball milling a single-phase strontium yttrium powder with isopropanol (isopropanol-1) and ball milling with other solvents (n-butanol-2, ethylene glycol-3, ethanol-4, methanol-5) (as a comparative example of the embodiment) (wherein the strontium yttrium yttrium standard card adopts JCPDF 74-0264). DETAILED DESCRIPTION

[0021] The following are specific embodiments and comparative examples of the present invention, combined with the accompanying drawings, to further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0022] Embodiment 1:

[0023] A method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0024] (1) mixing strontium oxalate and yttrium nitrate in a molar ratio of Sr:Y of 1:2;

[0025] (2) adding isopropanol to the mixture obtained in step (1) and ball milling at a speed of 4000 rpm, using a zirconia ball mill and a ball mill, and the ball milling time is 15 h;

[0026] (3) drying the slurry obtained in step (2) at 105° C. for 10 h;

[0027] (4) The powder obtained in step (3) is heat treated at 950° C. for 5 h to obtain strontium yttrium oxide powder.

[0028] Figure 1 The X-ray diffraction pattern (XRD) of the strontium yttrium powder synthesized by the present invention is kept at 950°C for 5 hours. The powder obtained by retrieval is strontium yttrium yttrium SrY2O4 single-phase composition JCPDS (PDF 74-0264).

[0029] Comparative Example 1:

[0030] A method for synthesizing a Y2O3-containing heterophase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0031] (1) mixing strontium oxalate and yttrium nitrate in a molar ratio of Sr:Y of 1:2;

[0032] (2) adding n-butanol to the mixture obtained in step (1) and ball milling the mixture at a speed of 4000 rpm, using a zirconia ball mill and a ball mill, and the ball milling time is 15 h;

[0033] (3) drying the slurry obtained in step (2) at 105° C. for 10 h;

[0034] (4) The powder obtained in step (3) is heat treated at 950° C. for 10 h to obtain a powder.

[0035] Figure 3 Spectrum No. 2 in the figure is the X-ray diffraction pattern (XRD) of the powder synthesized by using n-butanol as the ball milling medium and kept at 950°C for 10 hours. The powder obtained is retrieved to be strontium yttrium yttrium powder containing Y2O3 impurity phase (spectrum No. 1 is the XRD pattern of single-phase strontium yttrium yttrium powder without impurity phase).

[0036] Embodiment 2:

[0037] A method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0038] (1) mixing strontium carbonate and yttrium oxide in a molar ratio of Sr:Y of 1:2;

[0039] (2) adding isopropanol to the mixture obtained in step (1) and ball milling the mixture at a speed of 3000 rpm using a zirconia ball mill and a ball mill for 12 h;

[0040] (3) drying the slurry obtained in step (2) at 85° C. for 12 h;

[0041] (4) The powder obtained in step (3) is heat treated at 950° C. for 10 h to obtain strontium yttrium oxide powder.

[0042] Figure 2 The X-ray diffraction pattern (XRD) of the strontium yttrium powder synthesized by the present invention is kept at 950°C for 10 hours. The powder obtained by retrieval is strontium yttrium yttrium SrY2O4 single-phase composition JCPDS (PDF 74-0264).

[0043] Comparative Example 2:

[0044] A method for synthesizing a Y2O3-containing heterophase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0045] (1) mixing strontium carbonate and yttrium oxide in a molar ratio of Sr:Y of 1:2;

[0046] (2) adding ethylene glycol to the mixture obtained in step (1) and ball milling the mixture at a speed of 3000 rpm using a zirconia ball mill and a ball mill for 12 h;

[0047] (3) drying the slurry obtained in step (2) at 85° C. for 12 h;

[0048] (4) The powder obtained in step (3) is heat treated at 950° C. for 10 h to obtain a powder.

[0049] Figure 3 Spectrum No. 3 in the figure is the X-ray diffraction pattern (XRD) of the powder synthesized by using ethylene glycol as the ball milling medium and kept at 950°C for 10 hours. The powder obtained is retrieved to be strontium yttrium yttrium powder containing Y2O3 impurity phase (spectrum No. 1 is the XRD pattern of single-phase strontium yttrium yttrium powder without impurity phase).

[0050] Example 3

[0051] A method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0052] (1) mixing strontium acetate and yttrium oxide in a molar ratio of Sr:Y of 1:2;

[0053] (2) adding isopropanol to the mixture obtained in step (1) and ball milling the mixture at a speed of 4500 rpm, using a zirconium oxide spherical mill and a ball mill, and the ball milling time is 15 h;

[0054] (3) drying the slurry obtained in step (2) at 105° C. for 10 h;

[0055] (4) The powder obtained in step (3) is heat treated at 950° C. for 15 h to obtain strontium yttrium oxide powder.

[0056] Comparative Example 3:

[0057] A method for synthesizing a Y2O3-containing heterophase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0058] (1) mixing strontium acetate and yttrium oxide in a molar ratio of Sr:Y of 1:2;

[0059] (2) adding ethanol to the mixture obtained in step (1) and ball milling at a speed of 4500 rpm, using a zirconia ball mill and a ball mill, and the ball milling time is 15 h;

[0060] (3) drying the slurry obtained in step (2) at 105° C. for 10 h;

[0061] (4) The powder obtained in step (3) is heat treated at 950° C. for 10 h to obtain strontium yttrium oxide powder.

[0062] Figure 3 Spectrum No. 4 in the figure is the X-ray diffraction pattern (XRD) of the powder synthesized by using ethanol as the ball milling medium and kept at 950°C for 10 hours. The powder obtained is retrieved to be strontium yttrium yttrium powder containing Y2O3 impurity phase (spectrum No. 1 is the XRD pattern of single-phase strontium yttrium yttrium powder without impurity phase).

[0063] Example 4

[0064] A method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0065] (1) mixing strontium chloride and yttrium acetate in a molar ratio of Sr:Y of 1:2;

[0066] (2) adding isopropanol to the mixture obtained in step (1) and ball milling the mixture at a speed of 5000 rpm using a zirconia ball mill and a ball mill for 10 h;

[0067] (3) drying the slurry obtained in step (2) at 95° C. for 15 h;

[0068] (4) The powder obtained in step (3) is heat treated at 950° C. for 20 h to obtain strontium yttrium oxide powder.

[0069] Comparative Example 4:

[0070] A method for synthesizing a Y2O3-containing heterophase strontium yttrium oxide coating material by a low-temperature solid phase method comprises the following steps:

[0071] (1) mixing strontium chloride and yttrium acetate in a molar ratio of Sr:Y of 1:2;

[0072] (2) adding methanol to the mixture obtained in step (1) and ball milling the mixture at a speed of 5000 rpm, using a zirconia ball mill and a ball mill, and the ball milling time is 10 h;

[0073] (3) drying the slurry obtained in step (2) at 95° C. for 15 h;

[0074] (4) The powder obtained in step (3) is heat treated at 950°C for 10 hours to obtain strontium yttrium oxide powder.

[0075] Figure 3 Spectrum No. 5 in the figure is the X-ray diffraction pattern (XRD) of the powder synthesized using methanol as the ball milling medium and kept at 950°C for 10 hours. The powder obtained is retrieved to be strontium yttrium yttrium powder containing Y2O3 impurity phase (spectrum No. 1 is the XRD pattern of single-phase strontium yttrium yttrium powder without impurity phase).

[0076] For matters not mentioned above, the prior art applies.

[0077] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method, characterized in that: The steps include: (1) mixing a strontium salt and a yttrium salt or yttrium oxide in a molar ratio of Sr:Y of 1:2; (2) adding isopropanol to the mixture obtained in step (1) and performing high energy ball milling; (3) drying the slurry obtained in step (2); (4) The powder obtained in step (3) was heated at 950 o C temperature for 2 to 20 h to obtain single-phase SrY2O4 powder.

2. The method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method according to claim 1, characterized in that: The strontium salt in step (1) is any one of strontium carbonate, strontium oxalate, strontium nitrate, strontium chloride, strontium acetate or strontium sulfate.

3. The method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method according to claim 1, characterized in that: The yttrium salt in step (1) is any one of yttrium nitrate, yttrium chloride, yttrium sulfate or yttrium acetate.

4. The method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method according to claim 1, characterized in that: The ball milling parameters in step (2) are: rotation speed 2000-5000 rpm, zirconia ball mill and ball mill, and ball milling time 5-20 hours.

5. The method for synthesizing a single-phase strontium yttrium oxide coating material by a low-temperature solid phase method according to claim 1, characterized in that: Step (3) The slurry obtained in step (2) is heated at 80 to 105 o Dry at C for 10 to 24 hours.