A triptycene boron-nitrogen compound and its application

By using tributylene boron nitrogen compounds and stereostructure amine compounds modified with huge volume substituent triassene, the problems of current roll-off and high cost in OLED devices are solved, and a high efficiency and long-life TADF blue light luminescent material is achieved. , improves the performance of OLED devices.

CN115947747BActive Publication Date: 2024-11-26GUONENG PHOTOELECTRIC MATERIALS (SHENZHEN) CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310035335.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-10
Publication Date
2024-11-26
Estimated Expiration
2043-01-10

AI Technical Summary

Technical Problem

Existing organic semiconductor materials have current roll-off problems in OLED devices, resulting in reduced luminescence efficiency, and the use of precious metals increases costs and insufficient life, making it difficult to develop efficient, low-cost, and long-life blue light emitting materials.

Method used

The tributylene boron nitrogen compound modified with a large volume of substituent triassylene or its substitute is used to increase the solubility of the material and the transmission distance of the intermolecular excitons, thereby reducing the annihilation of the inversely luminescent molecules and increasing the current rolling of the OLED device. Reduce performance and reduce fluorescence quenching caused by intermolecular aggregation by more stereoscopic amine compounds.

Benefits of technology

It significantly reduces the current roll-off of OLED devices, improves luminous efficiency and life, especially in organic electroluminescent OLEDs, which significantly improves performance, and achieves high-efficiency and low-cost TADF blue light luminous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947747B_ABST
    Figure CN115947747B_ABST
Patent Text Reader

Abstract

The present invention provides a triptycene boron nitrogen compound and an application thereof. The triptycene boron nitrogen compound has a structure shown in Formula I. The triptycene boron nitrogen compound of the present invention can reduce the annihilation of excitons between luminescent molecules and reduce current roll-off when used as a light-emitting layer material of an OLED device. In particular, the current roll-off can be improved and the performance of the OLED device can be improved when used in an organic electroluminescent blue light OLED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic luminescent materials and relates to a triptycene boron nitrogen compound and an application of the same in an organic photoelectric device. Background Art

[0002] Organic semiconductor materials are new optoelectronic materials. Their large-scale research originated in 1977 when Hideki Shirakawa, A. Heeger and A. McDiamid jointly discovered doped polyacetylene with conductivity up to the level of copper. Subsequently, in 1987, C. Tang et al. of Kodak invented organic small molecule light-emitting diodes (OLEDs), in 1990 R. Friend and A. Holmes of Cambridge University invented polymer light-emitting diodes P-OLEDs, and in 1998 S. Forrest and M. Thomson invented more efficient organic phosphorescent light-emitting diodes PHOLEDs. Organic semiconductor materials have the advantages of easy structural adjustment, diverse varieties, adjustable energy bands, and even low cost like plastic film processing. In addition, organic semiconductors have been applied in many fields such as conductive films, electrostatic copying, photovoltaic solar cell applications, organic thin film transistor logic circuits, and organic light-emitting OLED flat panel displays and lighting. In 2000, Hideki Shirakawa, A. Heeger and A. McDiamid won the Nobel Prize in Chemistry.

[0003] As the organic electroluminescent diodes for the new generation of flat panel display applications, organic optoelectronic semiconductor materials require: 1. High luminous efficiency; 2. Excellent electron and hole stability; 3. Suitable luminescent color; 4. Excellent film processing; 5. Lower cost compared to liquid crystal displays. In principle, most conjugated organic molecules (including star emitters), conjugated polymers, and organic heavy metal complexes containing conjugated chromophore ligands have electroluminescent properties and are used in various types of light-emitting diodes, such as organic small molecule light-emitting diodes (OLEDs), polymer organic light-emitting diodes (POLEDs), organic phosphorescent light-emitting diodes (PHOLEDs), and organic thermally activated delayed fluorescence light-emitting diodes (TADF OLEDs). Organic phosphorescent light-emitting diodes use both singlet excited states (fluorescence) and triplet excited states (phosphorescence) to generate luminescent light, and have much higher luminous efficiency than small molecule OLEDs and polymer POLEDs. They have been used in many modern mobile phone displays, but the disadvantage is that they require the use of precious metals such as iridium or platinum, making OLED display phones expensive. Canon's staff first pioneered the use of triplet luminescent materials without precious metals in 2004 (US2006 / 0051616, US7749617), and obtained thermally activated delayed fluorescence (Thermally Activated Delayed Fluorescence) through reverse inter system crossing between triplet and singlet states, so that the excitons in the triplet state can emit fluorescence efficiently. Therefore, similar to phosphorescent triplet luminescent materials containing precious metals, the luminescence efficiency of TADF materials without precious metals is 3 to 4 times that of general fluorescent OLED materials, and the internal quantum efficiency can reach 100%. Therefore, TADF luminescent materials are expected to greatly reduce the cost of high-efficiency organic luminescent materials and increase the competitiveness of OLED display panels. As organic electroluminescent blue light emitting materials, phosphorescent triplet organic metal luminescent materials are 3 times more efficient than fluorescent luminescent materials, but due to life issues, current commercial AMOLEDs have to use fluorescent blue light materials with lower efficiency but relatively longer life. Therefore, the development of more stable and efficient electroluminescent blue light-emitting materials, especially the high-efficiency, low-cost and longer-lasting TADF blue light-emitting materials, has always been a strategically important topic in the industry.

[0004] In general organic semiconductor materials, according to Hound's rule, the energy of the triplet state is lower than that of the singlet state, and its energy band difference (△Es1-t1) is usually 0.6eV or more, making it basically impossible for electrons in the triplet state to return to the singlet state to emit light waves. In TADF materials, through molecular design, the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) in the molecular orbital have very little overlap, and fluorescent materials with a narrow energy level difference between the triplet and singlet states, even to only 0.3eV or less, are prepared, making it possible for electrons to cross from the triplet state to the singlet state (or RISC) and obtain an electroluminescent efficiency similar to 100% of phosphorescence.

[0005] In OLED devices, charge injection is achieved by injecting holes from the anode after applying a positive voltage to the anode, and injecting electrons after applying a negative voltage to the cathode. The electrons pass through the electron transport layer and the hole transfer layer, and enter the bulk material or the main material of the emission layer at the same time. The electrons eventually enter the lowest unoccupied molecular orbital (LUMO) of the luminescent dopant, and the holes enter the highest occupied molecular orbital (HOMO) of the luminescent dopant to form excited state luminescent dopant molecules (exciton state). After the exciton state returns to the ground state, it is accompanied by the emission of light energy, and the wavelength of the emitted light energy corresponds to the energy gap (HOMO-LUMO energy level difference) of the luminescent molecule dopant.

[0006] The prior art reports that multi-resonant boron-nitrogen compounds (Hatakeyama, et al, "Ultra pureblue thermally activated delayed fluorescencce molecules: Efficient HOMO-LUMOseparation by the multiple resonance effect" Adv. Mater., 2016, 28, 2777) have extremely narrow blue luminescence spectra. US20190058124 discloses the use of boron-containing organic semiconductors to obtain efficient blue luminescent materials, and the luminescence efficiency of OLED devices reaches or even exceeds that of organic metal iridium blue luminescent materials FIrPic. This type of boron-containing organic luminescent material has a triplet and singlet energy level difference of less than 0.4 eV, exhibiting RISC thermal delayed fluorescence TADF luminescence characteristics, and the polycyclic rings bonded by boron atoms present a plane, which is conducive to enhancing non-bonding orbital components, small vibration energy levels and shallow potential energy surfaces, suppressing bond energy vibration coupling, and achieving narrow spectrum luminescence. The emission wavelength can be in blue and green and the half-peak width of the spectrum is as small as 30nm. However, since the chromophore is connected by B and N, this p-π conjugation is essentially underdeveloped and its RISC (reverse system conversion rate) is low (less than 10 6 / s), resulting in low exciton utilization, and the multi-ring-shaped characteristics also cause a large roll-off in efficiency with increasing current density. US2022 / 0209123A1 discloses the use of developed chromophores such as naphthothiophene, but does not solve the problem of OLED light-emitting device efficiency roll-off with increasing current; EP3919500A1 discloses side chain alkane chain substitution and some bulky group substitution to achieve the purpose of improving luminous efficiency; CN202210502428 discloses the use of symmetrical phenylthiophene boron-nitrogen luminescent materials to improve lifespan. Increasing the proportion of guest materials in the light-emitting layer can reduce the problem of efficiency roll-off, but at the same time it will cause the light-emitting guest material to aggregate intermolecularly at higher doping concentrations (>10% by weight), resulting in reduced luminous efficiency.

[0007] Recently, the prior art reported the good steric effect of using triptycene, which is bonded to a symmetrical boron-nitrogen compound, but the blue-green light is involved, and the amines in the parent core structure are all planar condensed ring amines such as substituted carbazole, substituted acridine or substituted phenoloxazine, such as the following materials disclosed in CN202110932210:

[0008]

[0009] Obviously, in order to meet the ever-increasing performance requirements of industrial production, it is imperative to explore and obtain high-efficiency, low-cost, long-life organic OLED display and lighting products, and develop better, more efficient and easy-to-manufacture organic semiconductor materials. Summary of the invention

[0010] In view of the deficiencies in the prior art, the present invention aims to provide a triptycene boron nitrogen compound and its application.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In one aspect, the present invention provides a triptycene boron nitrogen compound, wherein the triptycene boron nitrogen compound has a structure shown in Formula I:

[0013]

[0014] wherein Ar1, Ar2 and Ar3 are each independently selected from a substituted or unsubstituted six- to twenty-membered aromatic ring, a substituted or unsubstituted six-membered aromatic heterocycle, a substituted or unsubstituted five-membered aromatic heterocycle, a bonded body of a substituted or unsubstituted five-membered or six-membered aromatic heterocycle having no more than 18 carbon atoms or a condensed aromatic heterocycle;

[0015] X1 and X2 are each independently selected from N-R5, O, S, Se, CR6R7 or SiR8R9;

[0016] R1, R2, R3, R4 and R5 are each independently at least one substitution satisfying the number of valence bonds (i.e., their respective number is at least one), and are independently selected from H, D (deuterium), F, Cl, substituted or substituted C1-C 30 Alkyl, substituted or unsubstituted C1-C 30 Alkoxy, -NR 10 R 11 , substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted C1-C 30 Alkylsilyl, substituted or unsubstituted C6-C 50 aromatic group, substituted or unsubstituted C3-C 50 Heteroaryl, substituted or unsubstituted C6-C 30 A fused heteroaryl group or a group containing a reactive unsaturated bond;

[0017] R6, R7, R8, R9, R 10 , R 11 Each is independently selected from a C1-C30 alkyl group, a C3-C30 cycloalkyl group, a substituted or unsubstituted C6-C50 aryl group, a substituted or unsubstituted C3-C50 heteroaryl group containing at least one heteroatom, a substituted or unsubstituted C6-C30 fused heteroaryl group or a group containing a reactive unsaturated bond.

[0018] When the above-mentioned group contains a substituent, the substituent is selected from H, D (deuterium), methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, phenyl, substituted phenyl, carbazolyl, substituted carbazolyl, thienyl, substituted thienyl, furyl, substituted furyl, selenophene, substituted selenophene, benzothienyl, substituted benzothienyl, phenylpropiofuranyl, substituted phenylpropiothienyl, phenylpropioselenophene, substituted phenylpropioselenophene, diphenylpropiothienyl, Substituted dibenzothienyl, dibenzofuranyl, substituted dibenzofuranyl, diphenylpropylselenol, substituted diphenylpropylselenol, wherein the substituent in the substituted group is selected from H, deuterium, F, Cl, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, cyano, phenyl, carbazolyl, thienyl, furyl, selenol, benzothienyl, phenylpropylfuranyl, phenylpropylselenol, diphenylpropylthienyl, dibenzofuranyl or diphenylpropylselenol.

[0019] After using the bulky substituent triazine or its substituent as a substitution in the triptycene boron nitrogen compound of the present invention, the material solubility is unexpectedly improved compared to the unsubstituted or other alkyl chain or aromatic heterocyclic substituted luminescent materials, reducing the aggregation of the luminescent guest material in the aggregated solid film, thereby reducing the current roll-off problem of the OLED device. The relaxation time of the exciton of the TADF luminescent material is generally in the microsecond and submicrosecond order, which is longer than that of the general fluorescent luminescent material (in the nanosecond order), or the intermolecular exciton transmission distance is longer. Therefore, most of the devices used for the main core material of the TADF luminescent material cannot meet the application of OLED luminescent display screens. The use of substituent modification becomes a topic related to whether the main core of the luminescent guest material can be applied. Through long-term research and development, the inventors found that the previous use of methyl, ethyl, tert-butyl or general cycloalkyl substitutions was difficult to effectively reduce the annihilation of excitons between luminescent molecules, while by using bulky substituents such as triazine or its substitutes, an outstanding modification effect can be achieved. Unexpectedly, it was found that the organic luminescent boron compounds substituted in this way can reduce the annihilation of excitons between luminescent molecules and reduce current roll-off, especially when applied to organic electroluminescent blue light OLEDs, to achieve improved current roll-off and improve OLED device performance.

[0020] The amines used in the compounds of the present invention are amines with a more stereoscopic structure, which are beneficial to reducing fluorescence quenching caused by intermolecular aggregation, thereby increasing device performance and reducing performance roll-off.

[0021] In the present invention, Ar1, Ar2 and Ar3 are each independently selected from any one of the following A1-A16 groups:

[0022]

[0023] The dotted line represents the connection position of the group, and Y is O, S, Se, SiR 14 R 15 or NR 14 R 15 , R 12 , R 13 , R 14 and R 15 At least one substitution to satisfy the number of valence bonds (i.e., the number of each is at least one) is independently selected from H, D (deuterium), F, Cl, substituted or unsubstituted C1-C30 alkyl, substituted or unsubstituted C1-C30 alkoxy, -NR1R2, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C1-C30 alkylsilyl, substituted or unsubstituted C6-C50 aryl, substituted or unsubstituted C3-C50 heteroaryl containing one or more heteroatoms, substituted or unsubstituted C6-C30 fused heteroaromatic or a group containing a reactive unsaturated bond.

[0024] Preferably, R1, R2, R3, R4 and R5 are each independently selected from H, D (deuterium), methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, phenyl, substituted phenyl, carbazolyl, substituted carbazolyl, thienyl, substituted thienyl, furyl, substituted furyl, selenophene, substituted selenophene, benzothienyl, substituted benzothienyl, phenylpropiofuranyl, substituted phenylpropiothienyl, phenylpropioselenophene, substituted phenylpropioselenophene, diphenylpropio Thienyl, substituted dibenzothienyl, dibenzofuranyl, substituted dibenzofuranyl, diphenylpropylselenol, substituted diphenylpropylselenol, wherein the substituent in the substituted group is selected from H, deuterium, F, Cl, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, cyclopentyl, hexyl, cyclohexyl, cyano, phenyl, carbazolyl, thienyl, furyl, selenol, benzothienyl, phenylpropylfuranyl, phenylpropylselenol, diphenylpropylthienyl, dibenzofuranyl or diphenylpropylselenol.

[0025] Preferably, the group containing a reactive unsaturated bond is a group containing a vinyl group, an acrylate group or a trifluorovinyl group.

[0026] In the present invention, the triptycene group in Formula I is connected to the structure in brackets by a line, which means that it can be connected to any connectable position on the structure in brackets, and it can be connected by a single bond or in a fused manner.

[0027] Preferably, the triptycene boron nitrogen compound is a compound having any one of the structures of Formula II to Formula VII:

[0028]

[0029]

[0030] Wherein X3 is selected from N-R5, O, S, Se, CR6R7 or SiR8R9, and X1, X2, Ar1, Ar2, Ar3, R1, R2, R3, R4, R5, R6, R7, R8, and R9 are the same as defined in Formula I.

[0031] Preferably, the triptycene boron nitrogen compound is any one of the following compounds:

[0032]

[0033]

[0034]

[0035]

[0036]

[0037]

[0038]

[0039]

[0040] Preferably, the triptycene boron nitrogen compound is any one of the following compounds:

[0041] In the present invention, the vinyl compounds in the triptycene boron nitrogen compounds X-1 to X-12 undergo chemical crosslinking reaction under heating to form an insoluble and infusible network crosslinked structure after crosslinking. For example, taking X-1 as an example, the crosslinking forms the following chain extension product:

[0042]

[0043] In the present invention, the acrylate compounds in the triptycene boron nitrogen compounds X-1 to X-12 undergo a cross-linking reaction when heated to 150° C. to form an insoluble and infusible cross-linked network structure. Taking compound X-2 as an example, the cross-linking forms the following chain extension product:

[0044]

[0045] In the present invention, the trifluoroethylene compounds in the triptycene boron nitrogen compounds X-1 to X-12 undergo a cross-linking reaction under heating conditions above 140° C. to form an insoluble and infusible cross-linked network structure. Taking compound X-3 as an example, the cross-linking forms the following chain extension products:

[0046]

[0047] In the present invention, the triptycene boron nitrogen compound can be prepared by the following preparation route:

[0048]

[0049] In another aspect, the present invention provides an organic semiconductor material, comprising at least one of the triptycene boron nitrogen compounds described above.

[0050] In another aspect, the present invention provides an organic light emitting diode, comprising a cathode, an anode and an organic thin film layer disposed between the cathode and the anode, wherein the organic thin film layer comprises the triptycene boron nitride compound as described above.

[0051] Preferably, the organic thin film layer comprises a light-emitting layer, the light-emitting layer comprises a host material and a guest material, and the guest material comprises the triptycene boron nitride compound as described above.

[0052] Preferably, the main material includes any one or a combination of at least two of the following materials:

[0053]

[0054] Preferably, the weight percentage content of the host material in the light-emitting layer is 85-99%, for example 85%, 88%, 90%, 93%, 95%, 98% or 99%, and the weight percentage content of the guest material is 1-15%, for example 1%, 3%, 5%, 8%, 10%, 12% or 15%.

[0055] In the present invention, in terms of OLED applications, an OLED light-emitting device generally includes: a base material, such as glass, metal foil, or polymer film; an anode, such as transparent conductive indium tin oxide; a cathode, such as conductive aluminum or other metals; one or more organic semiconductor layers (i.e., organic thin film layers), such as an electron injection layer between the light-emitting layer and the cathode, and a hole injection layer between the light-emitting layer and the anode, wherein the light-emitting layer contains a light-emitting dopant mixed with a main material to form a light-emitting layer. Usually, a light-emitting dopant material with a concentration (weight percentage) of 1-45% is used to be doped into the main material.

[0056] In the present invention, the triptycene boron nitrogen compound is used as a guest compound material of the light-emitting layer in an organic light-emitting diode, and is mixed with a host material (Host) or more than one host material to form a light-emitting layer. The triptycene boron nitrogen compound of the present invention is used as a light-emitting guest material (or dopant compound) and is mixed in a certain proportion in the host material to increase the efficiency of the light-emitting molecules, reduce self-quenching between the light-emitting dopant molecules and the change of the light-emitting color under different electric fields, and also reduce the amount of expensive light-emitting dopants. The mixed film can be formed by vacuum co-evaporation, or by mixing and dissolving in a solution and then spin-coating, spraying or solution printing.

[0057] In order to improve the luminous efficiency of the device, it is necessary to avoid the aggregation of luminescent molecules as much as possible. Usually, less than 50% by weight of the guest luminescent material (or dopant), preferably 1% to 40% of the dopant, is added to the host material. Of course, the host material can also be a mixed host material of more than one material, in which case the smaller amount is the auxiliary host material.

[0058] In the present invention, the triptycene boron nitrogen compound is used as a light-emitting layer material. Unlike charge transport materials that require the carrier mobility to be as large as possible, as a light-emitting material, avoiding quenching between molecules as much as possible is beneficial to improving the luminous efficiency and reducing the current roll-off when the device is working. Therefore, the triptycene boron nitrogen compound of the present invention uses asymmetric molecules as much as possible, and uses bulky triptycene or its substitutions, etc., to avoid the aggregation of multi-ring coplanar molecules. Table 1 lists the spatial effects produced by triptycene bonding to different multiple resonance luminescent guest materials. Figure 1A and Figure 1B Corresponding to the steric effect diagram of compound C-17, Figure 2A and Figure 2B Corresponding to the steric effect diagram of compound C-21, Figure 3A and Figure 3B Corresponding to the steric effect diagram of compound C-52, Figure 4A and Figure 4B Corresponding to the spatial effect diagram of compound C-39, according to the general formula of the present invention, these bulky substituents can be bonded to the ring connected by the polycyclic BN, or bonded to the side, especially the ortho position and meta position of the side. Compared with the general methyl, ethyl, propyl, butyl, tert-butyl and other substitutions, these substitutions are more effective in avoiding the annihilation or quenching of intermolecular excitons, thereby increasing the photoluminescence efficiency of the luminescent molecular material, reducing the current roll-off when the device is working, and ultimately improving the performance of the OLED device.

[0059] Table 1

[0060]

[0061]

[0062] The light-emitting device (or organic light-emitting diode) of the present invention contains the triptycene boron nitrogen compound of the present invention as a light-emitting dopant in the light-emitting layer, and forms the light-emitting layer with a host material by co-evaporation or solution co-coating; the thickness of the light-emitting layer is 12-60 nanometers, and the triplet energy level of the host material is 2.3-2.9eV, depending on the wavelength of the light emitted. If blue light is emitted, the triplet energy level of the host material should be greater than 2.75eV; if green light is emitted, the triplet energy level of the host material should be greater than 2.40eV; if red light is emitted, the triplet energy level of the host material should be greater than 2.15eV. One of the applications of the light-emitting material of the present invention is blue light with a light emission wavelength of 430-480nm, which is used as a TADF light-emitting dopant in the light-emitting layer of OLED.

[0063] The triptycene boron nitrogen compound molecules of the present invention contain an aromatic heterocyclic ring bonded with negative electronegativity boron and an aromatic amine ring bonded with electronegativity nitrogen, which have both electron-accepting and electron-donating bipolar natures and emit blue light of 440-480nm. Without violating the scope of the present invention, if a longer conjugated system is used, the luminescent material of the present invention can also be green light with a luminescent wavelength of 510-550nm, or yellow light of 551-580nm, or even red light of 581-630nm.

[0064] When green, yellow, and red light emitting materials with lower energy are mixed into the blue light emitting material, due to the energy transfer principle, the low energy material emits light first, while the higher energy blue light material only plays the role of the main material, or the role of luminescence sensitization. Therefore, the organic semiconductor of the present invention can obviously also be used as the main material of the green, yellow, and red light emitting OLED light emitting layer, that is, the light emitting layer contains the organic light emitting material of the present invention as the main material, and then other light emitting materials with longer wavelengths and lower energy are mixed to obtain application. When the light emitting layer thus constructed is injected with bidirectional charges, the generated excitons emit at the wavelength of the light emitting material with the lowest energy.

[0065] Preferably, the light-emitting layer comprises a host material, a guest material and a sensitizing material, and the sensitizing material comprises the triptycene boron nitrogen compound as described above.

[0066] In another case, the light-emitting layer can use a common host material and a common red, green or blue light-emitting dopant, and at the same time, the light-emitting layer is doped with a sensitizing material containing the triptycene boron nitrogen compound described in the present invention as an energy transfer. The semiconductor energy level of this sensitizing functional material is between the host material and the light-emitting dopant. According to the principle of energy transfer, the injected electrons and holes are successively transferred from the host material in the light-emitting layer to the sensitizing material and then to the light-emitting dopant. This step-by-step energy transfer can often increase the device life and increase the device efficiency.

[0067] In order to obtain efficient green and red OLEDs, triplet phosphorescent OLED materials or TADF luminescent materials using triplet emission mechanisms are usually used. The emission layer contains phosphorescent luminescent materials, such as Ir(ppy)3 for green light, or Ir(Piq)3 as a red light dopant, with 2 to 20% by weight of the luminescent material doped into a host material. Many other triplet red, green and even yellow luminescent materials have been developed in the literature or commercially, and can also be applied to the scope of the present invention.

[0068]

[0069] In order to obtain efficient blue light OLED, triplet phosphorescent OLED materials or TADF luminescent materials using triplet emission mechanism are usually used. The emission layer contains phosphorescent luminescent materials, such as the improved mFirPic, which has high luminescence efficiency, but the disadvantages are lifespan and color standard. While the use of fluorescent luminescent materials, such as B6, has an efficiency EQE of about 10%, but the lifespan and color standard can basically meet the current commercial AMOLED requirements.

[0070] Numerous other blue light emitting materials have been developed in the literature or commercially, and can also be applied to the scope of the present invention.

[0071]

[0072] In traditional organic light-emitting diode chips, transparent conductive glass or indium-tin oxide-plated ITO is usually used to evaporate a hole injection layer HIL, then a hole transport layer HTL, a light-emitting layer EML, an electron transport layer ETL, and an electron injection layer EIL are successively added, and finally a metal layer, such as an aluminum metal layer, is added as an anode conductive and sealing layer. When ITO is connected to positive electricity and aluminum is connected to negative electricity to a certain electric field, holes are injected from ITO through HIL and transferred to EML through HTL, while electrons are injected from EIL connected to aluminum and transferred to EML through ETL. Electrons and holes meet in EML and recombine into excitons, and then some excitons release energy in the form of light radiation and return to the ground state. The wavelength of the light radiation is determined by the energy gap of the luminescent dopant in the EML layer. Many other simple or more complex OLED light-emitting device structures have been developed in the literature or commercially, which can also be applied to the scope of the present invention.

[0073] The host material is usually a carbazole or aromatic amine structure material. A commonly used known host material is 4,4'-N,N'-dicarbazole-biphenyl (CBP):

[0074]

[0075] For TADF blue light OLED, the required electron injection and triplet energy level are relatively high, and the following DPEPO or mCBP materials are often used as the main materials:

[0076]

[0077] Preferably, the organic thin film layer further includes any one of a hole injection layer (HIL), a hole transport layer (HTL), an electron blocking layer (EBL), a hole blocking layer (HBL), an electron injection layer (EIL), and a combination of at least two of them.

[0078] In order to achieve excellent performance of the light-emitting device, a hole injection layer may be optionally provided on the anode. The material of the hole injection layer may be selected from, for example, CuPc or other aromatic amine-containing compounds (Appl. Phys. Lett., 69, 2160 (1996), such as m-TDATA.

[0079]

[0080] Similarly, a hole transport layer may be selected between the hole injection layer and the emission layer EML. The material of the hole transport layer may be 4,4′-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (α-NPD).

[0081]

[0082] In order to balance the injection of electrons and holes and improve the luminous efficiency, an electron transport hole blocking (ETHB) material can be selected, an example of which is 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene TPBi, whose structure is:

[0083]

[0084] An electron injection layer is usually used between the ETL and the cathode. The electron injection layer material is usually a metal lithium with a low work function, lithium fluoride or its compound such as 8-hydroxyquinoline lithium (Liq):

[0085]

[0086] Numerous other hole injection materials, hole transport materials, host materials, electron transport materials, electron injection materials, and exciton blocking materials have been developed in the literature or commercially, and can also be applied to the scope of the present invention.

[0087] OLED light-emitting devices are a complex multi-layer structure. Figure 5 It is a typical structure, but not the only applicable structure. The total thickness of the organic semiconductor layer is 50-250 nanometers, preferably 80-180 nanometers. The compounds of the present invention can be used in OLED complex multilayer light-emitting devices in principle, for example, using an exciton blocking layer between the light-emitting layer and the charge transport layer, including an electron transport hole blocking layer and a hole transport electron blocking layer, as long as the singlet and triplet states of the material are greater than the singlet and triplet states of the light-emitting material.

[0088] The triptycene boron nitrogen compound of the present invention generally belongs to the organic bonding composition of electronegative boron atoms and donor aromatic amines, wherein the boron-containing aromatic heterocycle responsible for electron injection dominates LUMO, and the aromatic heteroamine responsible for hole injection dominates HOMO, and Gaussian functional molecular calculation shows that HOMO and LUMO have little overlap, which is conducive to the generation of reverse system exchange (RISC) and the TADF luminescence mechanism, and obtains high efficiency of simultaneous singlet and triplet luminescence. Reverse system exchange (RISC) generally occurs between S1 and T1, and recent research progress shows that S1 and Tn (n is 2, 3, 4, etc.) may also be generated. The organic light-emitting layer compound disclosed in the present invention has a singlet and triplet energy level difference △E (S1-T1) of less than 0.2eV, and the fluorescence relaxation time is at the microsecond and sub-microsecond level, which is different from the fluorescence whose fluorescence relaxation time is at the nanosecond level. When applied to organic light-emitting diodes, an internal quantum efficiency exceeding 25% can be obtained, and a TADF light-emitting diode can be obtained. The organic semiconductor light-emitting material of the present invention has low cost, high charge transport and good processing performance, and is used to make organic light-emitting diodes to obtain improved high efficiency, low voltage and working life. Especially for TADF blue light materials, the improvement of life is a key progress in the industry.

[0089] The organic light emitting diode can be used as a light emitting dot matrix in a full-color OLED display screen, and the light emitting diode can be used as a blue light emitting device in a full-color OLED display screen. The light emitting diode can be used as a blue light emitting device combined with other light emitting devices to form a white light emitting device. In addition, since blue light has higher energy than green light and red light, the light emitting diode of the present invention can be used as a blue light emitting device to excite a green or red color film to obtain a full-color display application. The organic semiconductor compound in the organic light emitting diode is a sensitizing material for energy transfer in the light emitting layer. Changing the conjugated structure of the luminescent core can also become a green luminescent characteristic. After being improved with a special triphenylene substituent, it is also suitable for improving the characteristics of green BN luminescent materials.

[0090] The organic semiconductor material (i.e., triptycene boron nitrogen compound) of the present invention can be applied to organic light emitting diodes to obtain white light after adjusting the RGB three colors, and can be applied to OLED lighting. Using OLED flat screen display, it can be applied to mobile phone screens, i-Pack screens, TV screens, computer screens, etc., or as lighting luminous walls, luminous panels, luminous lamps, etc.

[0091] In another aspect, the present invention provides a display panel, comprising the organic light emitting diode as described above.

[0092] In the present invention, the organic light emitting diode can be used as a blue light emitting device in a full-color OLED display screen, or as a blue light emitting device combined with other light emitting devices to form a white light emitting device for use in a display screen, or as a blue light emitting device to excite a green or red color film to obtain a full-color display application.

[0093] Compared with the prior art, the present invention has the following beneficial effects:

[0094] The triptycene boron nitrogen compound of the present invention can be used as a light-emitting layer material of an OLED device to reduce the annihilation of excitons between light-emitting molecules and reduce current roll-off. In particular, when applied to an organic electroluminescent blue light OLED, the current roll-off can be improved and the performance of the OLED device can be enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0095] Figure 1A and Figure 1B This is the steric effect diagram of compound C-17.

[0096] Figure 2A and Figure 2B This is the steric effect diagram of compound C-21.

[0097] Figure 3A and Figure 3B This is the steric effect diagram of compound C-52.

[0098] Figure 4A and Figure 4B This is the steric effect diagram of compound C-39.

[0099] Figure 5 Schematic diagram of the structure of the OLED light-emitting device of the present invention, wherein 101 is an anode, 102 is a hole injection layer, 103 is a hole transport layer, 104 is a light-emitting layer, 105 is an electron transport layer, 106 is an electron injection layer, and 107 is a cathode.

[0100] Figure 6 The photoluminescence spectrum (PL) and electroluminescence spectrum (EL) of compound C-176 are shown in Figure 2. DETAILED DESCRIPTION

[0101] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0102] The organic semiconductor compound of the present invention can be prepared using a variety of synthetic routes, wherein a typical method can be implemented according to the following reaction route A:

[0103]

[0104] Reaction synthesis route A or route B:

[0105]

[0106] Reaction Synthesis Route B Example 1: Synthesis and Preparation of Compound C-113 Materials

[0107] Compound C-113 was prepared according to the following chemical synthesis route:

[0108]

[0109] 1) Synthesis of intermediate 5

[0110] In a 1000 ml three-necked flask, add the compound 3-bromo-5-(tert-butyl)benzo[B]thiophene (30 g, 111.44 mmol), p-tert-butylaniline (18.29 g, 122.58 mmol), tri(dibenzylideneacetone)dipalladium Pd2(dba)3 (1.02 g, 1.11 mmol), 4,5-bis(diphenylphosphine)-9,9-dimethylxanthene (XantPhos, 1.28 g, 2.22 mmol), sodium tert-butoxide (32.13 g, 334.32 mmol), and dry toluene (600 ml), and the reaction solution is refluxed under nitrogen protection for 6 h. The reaction solution was filtered through diatomaceous earth, rinsed with dichloromethane, and the solvent was dried under reduced pressure. After passing through a silica gel column (PE:DCM=5:1), a pink solid 1 (31.97 g, 85% yield) was obtained. The mass spectrum confirmed that it was consistent with the theoretical chemical formula C 22 H 27 NS (calculated Mol. Wt = 337.52, detected m / e = 337.2).

[0111] 2) Synthesis of intermediate 2:

[0112]

[0113] Anthracene (100 g, 0.56 mol), tert-butyl nitrite (115 g, 1.12 mol), and dry dichloromethane (500 mL) were added to a 2L three-necked flask to dissolve, and then a DME solution (300 mL) of 2-amino-5-bromobenzoic acid (363 g, 1.68 mol) was slowly added under reflux. The addition was completed in 4 hours, and the reaction was continued for 2 hours, and the reaction was stopped. The organic phase was concentrated and passed through a silica gel column (PE) to obtain a light yellow solid 2 (84 g, 45% yield), which was confirmed by mass spectrometry to be consistent with the theoretical chemical formula C 20 H 13 Br (calculated Mol. Wt = 333.22, detected m / e = 333.0).

[0114] 3) Synthesis of intermediate 3:

[0115]

[0116] Compound 2 (50 g, 0.15 mol), amine (40.6 g, 0.18 mol), Pd2(dba)3 (1.4 g, 1.5 mmol), XantPhos (1.7 g, 3.0 mmol), sodium tert-butoxide (43.2 g, 0.45 mol), and dry toluene (500 ml) were added to a 1000 ml three-necked flask, and the reaction solution was refluxed for 6 h under nitrogen protection. The reaction solution was filtered through diatomaceous earth, rinsed with dichloromethane, and the solvent was dried under reduced pressure. After passing through a silica gel column (PE: DCM = 5: 1), a white solid 3 (57 g, 80% yield) was obtained. The mass spectrum confirmed that it was consistent with the theoretical chemical formula C 36 H 31 N (calculated molecular weight Mol. Wt = 477.64, detected m / e = 277.2).

[0117] 4) Synthesis of intermediate 4:

[0118]

[0119] Compound 3 (55 g, 115 mmol), 3,5-dibromotoluene (57.5 g, 230 mmol), Pd2(dba)3 (1.1 g, 1.2 mmol), XantPhos (1.4 g, 2.4 mmol), sodium tert-butoxide (33.2 g, 345 mmol), and dry toluene (500 ml) were added to a 1000 ml three-necked flask, and the reaction solution was refluxed for 16 h under nitrogen protection. The reaction solution was filtered through diatomaceous earth, rinsed with dichloromethane, and the solvent was dried under reduced pressure. After silica gel column (PE), methanol was used for slurrying to obtain white solid 4 (55.8 g, 75% yield), which was verified by mass spectrometry to be consistent with the theoretical chemical formula C 43 H 36 BrN (calculated molecular weight Mol. Wt = 646.66, detected m / e = 645.2).

[0120] 5) Synthesis of intermediate 5:

[0121]

[0122] Compound 4 (55 g, 85 mmol), compound 1 (28.7 g, 85 mmol), Pd2(dba)3

[0123] (778 mg, 0.85 mmol), XantPhos (984 mg, 1.7 mmol), sodium tert-butoxide (24.5 g, 255 mmol), dry toluene (400 ml), the reaction solution was refluxed for 16 h under nitrogen protection. The reaction solution was filtered through diatomaceous earth, rinsed with dichloromethane, the solvent was dried under reduced pressure, and silica gel was passed through a column (PE: DCM = 10: 1) and then slurried with methanol to obtain a white solid 5 (49.9 g, 65% yield), which was confirmed by mass spectrometry to be consistent with the theoretical chemical formula C 65 H 62 N2S (calculated molecular weight Mol. Wt = 903.27, detected m / e = 902,5).

[0124] 5) Synthesis of compound C-176:

[0125]

[0126] Compound 5 (20 g, 22.14 mmol) and dried o-dichlorobenzene (220 ml) were added to a 250 ml three-necked flask, and nitrogen was replaced 3 times. BBr3 (4.3 ml, 44.28 mmol) was added at room temperature, and then the temperature was slowly raised to 145 ° C. After reacting for 3 hours, tert-butylbenzene was evaporated under reduced pressure, DCM was added to dissolve, and then concentrated and mixed with silica gel, passed through a silica gel short column (PE: DCM = 4: 1), and concentrated to obtain a crude product. Then, it was slurried with methanol and recrystallized with toluene to obtain 3 g of the product, a bright yellow solid, HPLC = 99.6%, a yield of 15%, and mass spectrometry confirmed that it was consistent with the theoretical chemical formula C 65 H 59 BNS (calculated molecular weight Mol. Wt = 911.05, detected m / e = 910.4).

[0127] Example 2: Synthesis and preparation of other compound materials

[0128] Similarly, according to the above synthetic chemistry principles, without violating the scope of the present invention, the following organic semiconductor light-emitting material compounds were synthesized. The molecular weights and molecular fragments of the compounds listed were verified by mass spectrometry, as shown in Table 4 below:

[0129] Table 4: Compound synthesis and characterization

[0130]

[0131]

[0132]

[0133] Example 3: Synthesis and preparation of cross-linkable compound materials

[0134] According to the general synthetic route, the following cross-linkable compound materials were synthesized by following the specific operation steps of Example 1. The molecular weight and fragment characterization were detected by MALDI-TOF mass spectrometry, which are listed in Table 5:

[0135] Table 5: Synthesis and characterization of cross-linkable compounds

[0136]

[0137]

[0138] Device Examples 1-10

[0139] The compound of the present invention is used as a light-emitting dopant material in an evaporation-deposited OLED device:

[0140] Evaporation OLED device process: the base vacuum reaches 10 -5 In the multi-source evaporation OLED preparation equipment of Pa, the following device structure is used: anode ITO / HIL / HTL / EBL(50A) / Host: luminescent dopant 1-40% / HBL(50A) / ET / EI / Al cathode; evaluate the performance of each material in OLED devices. The specific OLED device structure is ITO / HTACN / NPB / mCBP(50A) / H1 or H2: luminescent dopant 5% / Liq / TPBi / LiF / Al.

[0141] The selection of light-emitting layer materials in the device embodiments and comparative examples is shown in Table 7, wherein the comparative compounds Ref 1-4 used in comparative examples AD are shown in Table 6. The current-voltage-electroluminescence IVL and external quantum efficiency EQE of the device performance, and the accelerated aging life LT80% of the device (the time for the constant current brightness to drop by 20% at an initial brightness of 1000 nits) are tested.

[0142] The performance test results are shown in Table 6.

[0143] Table 6

[0144]

[0145] Table 7: OLED device performance obtained (room temperature @ 300 nits):

[0146]

[0147]

[0148] Among them, the comparative device A is the detection reference. At 1000 nits, the driving voltage is 5.2V, the external quantum efficiency EQE is 9.5%, the EL emission spectrum CIE (x, y) is (0.13, 0.11), and the life is LT80% = 90 hours at 1000 nits; the current roll-off index (maximum EQE and current increase to 1000 nits EQE efficiency ratio) of this material device is relatively large, which is 1.28. The current roll-off of the material device C without any substituent is 1.65, that is, after reaching 1000 nits brightness, its external quantum efficiency is reduced to 1 / 1.65 = 60.6% when it is at the maximum. The data in Table 7 take the voltage ratio and LT80% value of the comparative device A as 1, and the values ​​of other devices are relative values ​​relative to this device.

[0149] From the comparison of blue OLED devices A, B, C, and D in Table 7 above, it can be seen that the material of the present invention is used as a light-emitting material in blue OLED devices, which has the advantages of significantly improving the current roll-off of the material device and increasing the device life by 10-19%.

[0150] Device Embodiment

[0151] Application of cross-linkable luminescent materials in solution-coated OLED devices: On the surface of conductive glass ITO, after solvent and plasma cleaning, solution-spin-coat PEDOT conductive polymer as the hole injection layer HIL, use poly (triphenylamine-9.9-diheptanefluorene) solution spin-coated film as the hole transport layer HTL, and then use 5% of the cross-linkable luminescent materials X-1, X-4 and X-9 of the present invention and the main material solution (the main material is cross-linkable mCP, and the solvent is ethyl benzoate) to spin-coat the luminescent layer (main material 95%: luminescent dopant 5%). After heating to 160°C under nitrogen for 30 minutes, the EML layer is rinsed with xylene 10 times and then dried without weight loss, indicating that the film is cross-linked to become an infusible and insoluble luminescent layer EML; finally, the background vacuum reaches 10 -5 In the multi-source evaporation OLED preparation equipment of Pa, the BL layer, the electron transport layer ETL and the electron injection layer EIL were evaporated similarly to Example 4 to prepare the OLED device. The comparative experiment was that the solution was spin-coated with the light-emitting layer but the heating to 160°C for 30 minutes under nitrogen was not implemented, and the other steps were exactly the same. The results of the OLED devices showed that the initial OLED performance of the two was similar, and the life of the OLED devices after thermal cross-linking increased by 18%, 20% and 19% respectively; the current roll-off index was less than 1.15.

[0152] The applicant declares that the present invention illustrates the triptycene boron nitrogen compound and its application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A triptycene boron-nitrogen compound, characterized in that: The triptycene boron nitrogen compound is a compound having any one of the structures of Formula II to Formula VII: Ar1 is selected from the following groups: Ar2 and Ar3 are each independently selected from any one of the following groups: The dotted line represents the connection position of the group, Y is S, R 12 At least one substitution to satisfy the number of valence bonds is independently selected from H or D; X1 is selected from N-R5 or S; X2 is selected from N-R5; wherein X3 is selected from S; R1, R2, R3, R4 and R5 are each independently selected from H, D, methyl, isopropyl, tert-butyl, phenyl or substituted phenyl, wherein the substituent in the substituted group is selected from H, deuterium, methyl, tert-butyl, cyclopentyl or phenyl.

2. A triptycene boron-nitrogen compound, characterized in that: The triptycene boron nitrogen compound is any one of the following compounds:

3. A triptycene boron-nitrogen compound, characterized in that: The triptycene boron nitrogen compound is any one of the following compounds:

4. An organic light emitting diode, characterized in that: The organic light emitting diode comprises a cathode, an anode and an organic thin film layer arranged between the cathode and the anode; The organic thin film layer comprises a light-emitting layer, the light-emitting layer comprises a host material and a guest material, and the guest material comprises the triptycene boron nitrogen compound according to any one of claims 1 to 3.

5. The organic light emitting diode according to claim 4, characterized in that: The main material includes any one or a combination of at least two of the following materials:

6. The organic light emitting diode according to claim 4, characterized in that: The weight percentage of the host material in the light-emitting layer is 85-99%, and the weight percentage of the guest material is 1-15%.

7. The organic light emitting diode according to claim 4, characterized in that: The organic thin film layer further comprises any one of a hole injection layer, a hole transport layer, an electron blocking layer, a hole blocking layer, an electron injection layer or an electron injection layer, or a combination of at least two thereof.

8. A display panel, characterized in that: The display panel includes the organic light emitting diode as claimed in claim 4.