A method for loading high-content platinum on carbon aerogel

By using ball milling technology with PEG-100 and specific grinding ball ratios, combined with loading method, the problem of improving the total specific surface area and mesoporosis of carbon aerogel is solved, and the specific surface area and mesoporosis of high-content platinum catalysts are synchronously improved. Improves the performance of platinum catalyst.

CN115954492BActive Publication Date: 2024-11-19SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211600914.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-19
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

In the prior art, the total specific surface area and mesoporosis of carbon aerogels are difficult to synchronously improve, which affects the performance of the electrocatalyst.

Method used

The specific surface area and mesoporosis of carbon aerogels are improved through the ball milling process by using a specific pore-forming agent PEG-100 and a specific ball-milling ratio (bead mass ratio of 10mm, 5mm and 2mm diameters). , combined with specific loading methods such as ultrasonic dispersion and ultraviolet reduction, carbon aerogel catalysts with high platinum content were prepared.

Benefits of technology

The specific surface area of ​​the carbon aerogel reached 1029.95m2/g and the mesoporosis reached 92.18%, which simultaneously increased the total specific surface area and mesoporosis, and improved the loading and dispersion of the platinum catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115954492B_ABST
    Figure CN115954492B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for loading high-content platinum on carbon aerogel, and relates to the technical field of electrocatalyst material preparation. Based on the prior art, the present invention uses a specific pore-forming agent PEG-100 and sets a specific grinding ball ratio (the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1). Although the technical changes are not significant, the carbon aerogel loaded with high content of platinum has obvious improvements: its specific surface area is up to 1029.95 m 2 / g, the pore size distribution is between 10 and 18 nm, and the mesoporosity reaches 92.18%, achieving a simultaneous increase in the total specific surface area and mesoporosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrocatalyst material preparation, and in particular to a method for loading high-content platinum on carbon aerogel. Background Art

[0002] Platinum catalyst is a general term for catalysts made of metal platinum as the main active ingredient, and commonly used carriers are carbon black, aluminum oxide, etc. It has the characteristics of high catalytic activity and strong selectivity, and has a wide range of applications. It is mainly used in chemical reactions such as hydrogen oxidation, methanol oxidation, formic acid oxidation and oxygen reduction in fuel cells. It is a very common precious metal catalyst.

[0003] Platinum catalysts used in hydrogen fuel cells generally have a platinum loading of more than 20%. In addition, platinum catalysts used in hydrogen fuel cells require platinum nanoparticles with small particle size, narrow particle size distribution, uniform dispersion on the carrier, and no harmful impurities (such as Cl - Since the surface energy of small-sized platinum nanoparticles is very large and they are easy to agglomerate, it is very difficult to prepare platinum catalysts with small platinum nanoparticles, narrow particle size distribution, and uniform dispersion on the carrier.

[0004] The 2020 dissertation of our research group, "Application of Platinum@Carbon Aerogel in Aluminum-Air Batteries", uses carbon aerogel with high porosity and high specific surface area to load high content of platinum. The preparation process of the carbon aerogel includes the following steps:

[0005] (1) A certain amount of phloroglucinol, resorcinol and formaldehyde are dissolved in ultrapure water to prepare a PRF precursor solution.

[0006] (2) Pour the prepared precursor solution into a flask containing white oil and surfactant Span 80, wherein the volume ratios of white oil to Span 80 and precursor solution are 100:1 and 10:1, respectively. Then, the mixed solution is stirred at a high speed of 1000 r / min for 30 min, and then the stirring speed is reduced to 200 r / min, and the mixture is reacted at 60°C for 12 h. Span 80 as a surfactant is mixed with white oil and stirred at high speed to form a large number of small bubbles. The precursor solution enters the small bubbles during the high-speed stirring process, thereby forming an inverse suspension microemulsion.

[0007] (3) After the above reaction is completed, the mixed solution is poured into a sand core funnel for filtration and repeatedly rinsed with dichloromethane. The obtained powder solid is placed in a ventilated place indoors for 2 days, and then dried in a forced air drying oven at 60°C for 24 hours to obtain hydrogel microspheres. Since the sol-gel reaction process in the precursor solution is carried out in a microemulsion, hydrogel microspheres are obtained after the gel is completed.

[0008] (4) The hydrogel microspheres prepared in step (3) were placed in a tubular furnace and carbonized at 950° C. for 4 h under nitrogen protection to obtain carbon aerogel microspheres (CPRF).

[0009] (5) The carbon aerogel microspheres prepared in step (4) are placed in a tubular furnace and activated with CO2 at 950°C for 3 h to obtain activated carbon aerogel microspheres (ACPRF).

[0010] Then, carbon aerogel microspheres (CPRF) and activated carbon aerogel microspheres (ACPRF) were ball-milled and loaded with platinum. However, according to the pore size distribution diagram, specific surface area and pore volume data, it is not difficult to know that although ACPRF has a higher total specific surface area than CPRF, it may be because it produces a large number of micropores (pore size 1-4nm) that are not conducive to charge transfer and platinum catalytic performance. Therefore, how to further improve the total specific surface area, mesoporosity and other data of carbon aerogel microspheres simultaneously is crucial for the development of electrocatalyst materials. Summary of the invention

[0011] In view of the above problems in the prior art, the present invention provides a method for loading high-content platinum on carbon aerogel to solve the technical problem of the contradiction between the total specific surface area and the mesoporosity of carbon aerogel in the prior art.

[0012] The technical solution adopted by the present invention is as follows:

[0013] A method for loading high-content platinum on carbon aerogel comprises the following steps:

[0014] (1) Add white oil and Span 80 in a ratio of 100:1 into a three-necked flask to form solvent A, and continue stirring;

[0015] (2) dissolving phloroglucinol and resorcinol with formaldehyde, wherein the molar ratio of phloroglucinol to resorcinol is 1:7, and the molar ratio of the total molar ratio of resorcinol and phloroglucinol to formaldehyde is 1:2, and adding ultrapure water thereto to form a light yellow transparent solution B, wherein the volume of the solution B is 10% of the volume of the solvent A;

[0016] (3) adding 1% by weight of PEG-100 to solution B to form precursor solution C;

[0017] (4) Precursor solution C is added to solvent A, stirred evenly, and reacted in an oil bath at 60-80° C. for 10-15 hours while stirring. The obtained turbid reaction solution is filtered and rinsed with dichloromethane. The obtained non-agglomerated powdery orange-yellow solid is allowed to stand at room temperature and pressure for 3 days, then air-dried at 80-100° C. for 10-15 hours, taken out, and carbonized at 950° C. under nitrogen protection for 4 hours to obtain carbon aerogel;

[0018] (5) placing the carbon aerogel obtained in step (4) in a ball mill, and placing zircon ball milling beads in the ball mill, wherein the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1, and during the ball milling process, adding a small amount of ethanol and mixing evenly, and then ball milling for 60 minutes, adjusting the ball milling frequency to 45 Hz, and taking out after the ball milling is completed and drying in a vacuum environment at 60 to 80° C. for 10 to 15 hours to obtain carbon aerogel powder;

[0019] (6) Platinum is loaded on carbon aerogel powder.

[0020] Preferably, in step (5), the mass ratio of the added amount of the carbon aerogel to the ball milling beads is 1:650.

[0021] Preferably, in step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: sodium borohydride is dissolved in ultrapure water to prepare a sodium borohydride solution and poured into a separatory funnel for standby use; chloroplatinic acid aqueous solution and the carbon aerogel powder obtained in step (5) are added to ultrapure water, and a precursor solution is formed after ultrasonic dispersion; the sodium borohydride solution is added dropwise to the precursor solution while stirring, and stirring is maintained for 10 to 15 hours after the addition is completed, and then the reaction solution is filtered, rinsed with ultrapure water, and the filter cake is dried in a vacuum environment at 60 to 80° C. for 10 to 15 hours to obtain a carbon aerogel-loaded platinum catalyst.

[0022] Preferably, in step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: take the ball-milled carbon aerogel powder and place it in a culture dish, spread it evenly, drop chloroplatinic acid solution into it and disperse it evenly by ultrasonication, and put it together with the culture dish into a UV curing furnace for UV reduction to obtain a carbon aerogel-loaded platinum catalyst.

[0023] More preferably, in the ultraviolet reduction operation, the illumination time is set to 85 minutes and the illumination power is set to 100%.

[0024] Preferably, in step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: adding chloroplatinic acid solution to ethylene glycol, adjusting the pH to 13 with sodium hydroxide solution, and then adding ball-milled carbon aerogel powder, and forming a precursor solution after ultrasonic dispersion; pouring the precursor solution into a three-necked flask and carrying out an oil bath at 130° C. for 4 hours, cooling to room temperature and slowly adding concentrated acid dropwise until the pH is less than 3, maintaining stirring for 12 hours, then filtering the reaction solution, first rinsing with acetone and then rinsing with ultrapure water, and drying the filter cake in a vacuum environment at 60-80° C. for 10-15 hours to obtain a carbon aerogel-loaded platinum catalyst.

[0025] In summary, compared with the prior art, the present invention has the following advantages and beneficial effects:

[0026] The present invention uses a specific pore-forming agent PEG-100 and sets a specific grinding ball ratio (the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1), and finally obtains a carbon aerogel loaded with high platinum content, whose specific surface area reaches up to 1029.95 m 2 / g, the pore size is mainly distributed in the range of 10-18nm, and the mesoporosity reaches 92.18%, achieving a simultaneous increase in the total specific surface area and mesoporosity. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a nitrogen adsorption-desorption curve of the carbon aerogel-supported platinum catalyst obtained in Example 1;

[0028] Figure 2 This is the pore size distribution diagram of the carbon aerogel-supported platinum catalyst obtained in Example 1;

[0029] Figure 3 This is a transmission electron microscopy image of the carbon aerogel-supported platinum catalyst obtained in Example 1;

[0030] Figure 4 The nitrogen adsorption-desorption curves of the carbon aerogel-supported platinum catalyst obtained by various parameters in Comparative Example 1 are shown in FIG. 1 , where a represents PEG-200, b represents PEG-400, c represents PEG-600, and d represents PEG-800;

[0031] Figure 5 The pore size distribution diagram of the carbon aerogel-supported platinum catalyst obtained by various parameters in Comparative Example 1, in which a represents PEG-200, b represents PEG-400, c represents PEG-600, and d represents PEG-800;

[0032] Figure 6 Transmission electron microscopy images of the carbon aerogel-supported platinum catalyst obtained with various parameters in Comparative Example 1.

[0033] Figure 7 The nitrogen adsorption-desorption curves of the carbon aerogel-supported platinum catalyst obtained by various parameters in Comparative Example 2, in which e / f / g / h / i / j / k / l represent different ball milling parameters in Table 2 respectively;

[0034] Figure 8 The pore size distribution diagram of the carbon aerogel-supported platinum catalyst obtained by various parameters in Comparative Example 2, in which e / f / g / h / i / j / k / l represent different ball milling parameters in Table 2 respectively;

[0035] Fig. 9 The transmission electron microscopy image of the carbon aerogel-supported platinum catalyst obtained by various parameters in Comparative Example 2;

[0036] Fig.10 This is a nitrogen adsorption-desorption curve of the carbon aerogel-supported platinum catalyst obtained in Example 2;

[0037] Fig.11 This is the pore size distribution diagram of the carbon aerogel-supported platinum catalyst obtained in Example 2;

[0038] Fig.12 This is a transmission electron microscopy image of the carbon aerogel-supported platinum catalyst obtained in Example 2;

[0039] Fig.13 This is a nitrogen adsorption-desorption curve of the carbon aerogel-supported platinum catalyst obtained in Example 3;

[0040] Fig.14 This is the pore size distribution diagram of the carbon aerogel-supported platinum catalyst obtained in Example 3;

[0041] Fig.15 This is a transmission electron microscopy image of the carbon aerogel-supported platinum catalyst obtained in Example 3. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and various embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.

[0043] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this method adopt conventional test methods in the art. The terms described in the present invention are only for describing specific implementation methods and are not intended to limit the content disclosed in the present invention.

[0044] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the invention belongs; other raw materials, reagents, experimental methods and technical means not specifically specified in the present invention refer to the raw materials and reagents commonly used by ordinary technicians in the field, as well as the commonly used experimental methods and technical means.

[0045] Example 1

[0046] This embodiment provides a specific example of carbon aerogel loaded with high content of platinum:

[0047] Step 1: Preparation of carbon aerogel. Add white oil: Span 80 = 100:1 into a three-necked flask to form solvent 1, stir at 1000 rpm for 30 minutes, adjust to 600 rpm and continue stirring. Take phloroglucinol and resorcinol and dissolve them with formaldehyde (wherein, the molar ratio of phloroglucinol and resorcinol is 1:7, and the molar ratio of formaldehyde to the total amount of resorcinol is 2:1), add ultrapure water to 10% of the volume of solvent 1 to obtain a light yellow transparent solution, and then add PEG-100 (polyethylene glycol-100) with a mass of 1% of the total mass of the light yellow transparent solution to form a precursor solution. Add the precursor solution to solvent 1, stir evenly, and react in a 60°C oil bath while stirring for 12 hours. The turbid reaction liquid was filtered and rinsed with dichloromethane. The obtained non-agglomerated powdery orange-yellow solid was allowed to stand at room temperature and pressure for 3 days, dried with air at 80°C for 12 hours, and carbonized at 950°C under nitrogen protection for 4 hours to obtain carbon aerogel.

[0048] Step 2: Ball milling of carbon aerogel. Put zircon ball milling beads (wherein the mass ratio of beads with diameters of 10mm, 5mm, and 2mm is 2:10:1) in a ball milling jar, add carbon aerogel with a mass ratio of 1:650 to ball milling beads, drop a small amount of ethanol and mix well, then ball mill for 60 minutes, and adjust the ball milling frequency to 45Hz (Hertz). After the ball milling is completed, take out and dry in a vacuum environment at 60℃ for 12 hours to obtain a carbon aerogel powder carrier material.

[0049] Step 3: Platinum loading. Take 23-60 mg of sodium borohydride and dissolve it in 30 mL of ultrapure water to make a sodium borohydride solution and pour it into a separatory funnel for use. Add chloroplatinic acid aqueous solution (mass fraction 8wt%, volume 500-1250μL) and 40-80 mg of ball-milled carbon aerogel powder to 50 mL of ultrapure water, and form a precursor solution after ultrasonic dispersion. While stirring, add the sodium borohydride solution drop by drop into the precursor solution, and maintain the stirring speed of 600 rpm for 12 hours after the dripping. Then filter the reaction solution, rinse it with 200 mL of ultrapure water, take the filter cake and dry it in a vacuum environment at 60°C for 12 hours to obtain a carbon aerogel-loaded platinum catalyst (Pt@CA).

[0050] The total specific surface area of ​​the carbon aerogel-supported platinum catalyst obtained in this example is 1029.95 m 2 / g, the pore size is mainly distributed in the range of 10 to 18 nm, the mesoporosity reaches 92.18%, and the ICP-OES (inductively coupled plasma emission spectrometer) test proves that the carbon aerogel-supported platinum catalyst obtained in this embodiment can be efficiently loaded, with a theoretical loading of 50% and an actual loading of 47.90%. TEM (transmission electron microscopy) observation shows that the loaded platinum metal particles are small and uniformly dispersed, with a particle size distribution of 1.5 to 2.0 nm.

[0051] Comparative Example 1

[0052] On the basis of Example 1, only PEG-100 was replaced by PEG-200, PEG-400, PEG-600, and PEG-800, respectively.

[0053] The total specific surface area and mesoporosity data of the carbon aerogel-supported platinum catalyst obtained in Example 1 and Comparative Example 1 are shown in Table 1.

[0054] Table 1 Specific surface area and mesoporosity of carbon aerogels prepared from different raw materials before and after ball milling

[0055] project PEG-100 PEG-200 PEG-400 PEG-600 PEG-800 <![CDATA[S tot (m 2 .g -1 )]]> 1029.95 867.48 878.37 851.47 840.45 Mesoporosity (%) 92.18 80.34 81.53 79.81 86.44

[0056] Comparative Example 2

[0057] On the basis of Example 1, only the ball milling parameters were changed to have mass ratios of beads with diameters of 10 mm, 5 mm, and 2 mm of 1:10:1, 1:10:0, 10:0:1, 0:10:1, 10:0:0, 0:10:0, and 0:0:10, respectively.

[0058] The total specific surface area and mesoporosity data of the carbon aerogel-supported platinum catalyst obtained in Example 1 and Comparative Example 2 are shown in Table 2.

[0059] Table 2 Specific surface area and mesoporosity of carbon aerogels prepared with different ball milling parameters before and after ball milling

[0060] project <![CDATA[S tot (m 2 .g -1 )]]> Mesoporosity (%) e: Specifications: 10mm, 5mm, 2mm, mass ratio is 2:10:1 1029.95 92.18 f: Specifications: 10mm, 5mm, 2mm, mass ratio is 1:10:1 930.78 88.06 g: Specifications: 10mm, 5mm, 2mm, mass ratio is 1:10:0 873.17 83.63 h: Specifications: 10mm, 5mm, 2mm, mass ratio: 10:0:1 750.75 78.11 i: Specifications: 10mm, 5mm, 2mm, mass ratio: 0:10:1 878.89 85.29 j: Specifications: 10mm, 5mm, 2mm, mass ratio: 10:0:0 744.30 78.85 k: Specifications: 10mm, 5mm, 2mm, mass ratio: 0:10:0 859.65 82.48 l: Specifications: 10mm, 5mm, 2mm, mass ratio: 0:0:10 754.99 74.73

[0061] Example 2

[0062] This embodiment provides a specific example of carbon aerogel loaded with high content of platinum:

[0063] Step 1: Preparation of carbon aerogel. Add white oil: Span 80 = 100:1 into a three-necked flask to form solvent 1, stir at 1000 rpm for 30 minutes, adjust to 600 rpm and continue stirring. Take phloroglucinol and resorcinol and dissolve them with formaldehyde (wherein, the molar ratio of phloroglucinol and resorcinol is 1:7, and the molar ratio of formaldehyde to the total amount of resorcinol is 2:1), add ultrapure water to 10% of the volume of solvent 1 to obtain a light yellow transparent solution, and then add PEG-100 (polyethylene glycol-100) with a mass of 1% of the total mass of the light yellow transparent solution to form a precursor solution. Add the precursor solution to solvent 1, stir evenly, and react in a 60°C oil bath while stirring for 12 hours. The turbid reaction liquid was filtered and rinsed with dichloromethane. The obtained non-agglomerated powdery orange-yellow solid was allowed to stand at room temperature and pressure for 3 days, dried with air at 80°C for 12 hours, and carbonized at 950°C under nitrogen protection for 4 hours to obtain carbon aerogel.

[0064] Step 2: Ball milling of carbon aerogel. Place zircon ball milling beads (wherein the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1) in a ball milling jar, add carbon aerogel with a mass ratio of 1:650 to ball milling beads, drop a small amount of ethanol and mix well, then ball mill for 60 minutes, and adjust the ball milling frequency to 45 Hz (Hertz). After the ball milling is completed, take out and dry in a vacuum environment at 60°C for 12 hours to obtain a carbon aerogel powder carrier material.

[0065] Step 3: Platinum loading. Take 40-80 mg of ball-milled carbon aerogel powder and place it in a 60 mm culture dish, spread it evenly, drop chloroplatinic acid solution into it and disperse it evenly by ultrasonication, and place it together with the culture dish into a UV curing oven for UV reduction, set the illumination time to 85 minutes, the illumination power to 100%, and take it out after one illumination to obtain the carbon aerogel-loaded platinum catalyst (Pt@CA).

[0066] The total specific surface area of ​​the carbon aerogel-supported platinum catalyst obtained in this example is 1018.44 m 2 / g, the pore size is mainly distributed in 8-20nm, and the mesoporosity reaches 91.11%. The ICP-OES (inductively coupled plasma emission spectrometer) test proves that the carbon aerogel-supported platinum catalyst obtained in this embodiment can be efficiently loaded, with a theoretical loading of 50% and an actual loading of 48.70%. The TEM (transmission electron microscope) observation shows that the loaded platinum metal particles are small and uniformly dispersed, with a particle size distribution of 1.5-2.0nm.

[0067] Example 3

[0068] This embodiment provides a specific example of carbon aerogel loaded with high content of platinum:

[0069] Step 1: Preparation of carbon aerogel. Add white oil: Span 80 = 100:1 into a three-necked flask to form solvent 1, stir at 1000 rpm for 30 minutes, adjust to 600 rpm and continue stirring. Take phloroglucinol and resorcinol and dissolve them with formaldehyde (wherein, the molar ratio of phloroglucinol and resorcinol is 1:7, and the molar ratio of formaldehyde to the total amount of resorcinol is 2:1), add ultrapure water to 10% of the volume of solvent 1 to obtain a light yellow transparent solution, and then add PEG-100 (polyethylene glycol-100) with a mass of 1% of the total mass of the light yellow transparent solution to form a precursor solution. Add the precursor solution to solvent 1, stir evenly, and react in a 60°C oil bath while stirring for 12 hours. The turbid reaction liquid was filtered and rinsed with dichloromethane. The obtained non-agglomerated powdery orange-yellow solid was allowed to stand at room temperature and pressure for 3 days, dried with air at 80°C for 12 hours, and carbonized at 950°C under nitrogen protection for 4 hours to obtain carbon aerogel.

[0070] Step 2: Ball milling of carbon aerogel. Place zircon ball milling beads (wherein the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1) in a ball milling jar, add carbon aerogel with a mass ratio of 1:650 to ball milling beads, drop a small amount of ethanol and mix well, then ball mill for 60 minutes, and adjust the ball milling frequency to 45 Hz (Hertz). After the ball milling is completed, take out and dry in a vacuum environment at 60°C for 12 hours to obtain a carbon aerogel powder carrier material.

[0071] Step 3: Platinum loading. Add chloroplatinic acid solution to ethylene glycol, adjust pH>13 with 1 mol / L (mole per liter) sodium hydroxide solution, then add ball-milled carbon aerogel powder (wherein the volume of ethylene glycol is 50-100 mL, the mass of carbon aerogel powder is 40-80 mg, and the volume of chloroplatinic acid solution with a mass fraction of 8wt% is 500-1250 μL), and form a precursor solution after ultrasonic dispersion. Pour the precursor solution into a three-necked flask and place it in an oil bath at 130°C for 4 hours. After cooling to room temperature, slowly add concentrated acid until pH<3 (concentrated acid includes hydrochloric acid, nitric acid, sulfuric acid, etc.), and stir at a speed of 600 rpm for 12 hours. Then filter the reaction solution, rinse it with acetone first and then with ultrapure water, take the filter cake and dry it in a vacuum environment at 60°C for 12 hours to obtain a carbon aerogel-loaded platinum catalyst (Pt@CA).

[0072] The total specific surface area of ​​the carbon aerogel-supported platinum catalyst obtained in this example is 1025.42 m 2 / g, the pore size is mainly distributed in 8-21nm, and the mesoporosity reaches 90.79%. The ICP-OES (inductively coupled plasma emission spectrometer) test proves that the carbon aerogel-supported platinum catalyst obtained in this embodiment can be efficiently loaded, with a theoretical loading of 50% and an actual loading of 48.70%. The TEM (transmission electron microscope) observation shows that the loaded platinum metal particles are small and uniformly dispersed, with a particle size distribution of 1.5-2.0nm.

[0073] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for loading high-content platinum on carbon aerogel, characterized in that: The steps include: (1) Add white oil and Span 80 in a ratio of 100:1 into a three-necked flask to form solvent A, and continue stirring; (2) dissolving phloroglucinol and resorcinol with formaldehyde, wherein the molar ratio of phloroglucinol to resorcinol is 1:7, and the molar ratio of the total molar ratio of resorcinol and phloroglucinol to formaldehyde is 1:2, and adding ultrapure water thereto to form a light yellow transparent solution B, wherein the volume of the solution B is 10% of the volume of the solvent A; (3) adding 1% by weight of PEG-100 to solution B to form precursor solution C; (4) Precursor solution C is added to solvent A, stirred evenly, and reacted in an oil bath at 60-80° C. for 10-15 hours while stirring. The obtained turbid reaction solution is filtered and rinsed with dichloromethane. The obtained non-agglomerated powdery orange-yellow solid is allowed to stand at room temperature and pressure for 3 days, then air-dried at 80-100° C. for 10-15 hours, taken out, and carbonized at 950° C. under nitrogen protection for 4 hours to obtain carbon aerogel; (5) placing the carbon aerogel obtained in step (4) in a ball mill, and placing zircon ball milling beads in the ball mill, wherein the mass ratio of beads with diameters of 10 mm, 5 mm, and 2 mm is 2:10:1, and during the ball milling process, adding a small amount of ethanol and mixing evenly, and then ball milling for 60 minutes, adjusting the ball milling frequency to 45 Hz, and taking out after the ball milling is completed and drying in a vacuum environment at 60 to 80° C. for 10 to 15 hours to obtain carbon aerogel powder; (6) Platinum is loaded on carbon aerogel powder.

2. The method for loading high-content platinum on carbon aerogel according to claim 1, characterized in that: In step (5), the mass ratio of the added amount of the carbon aerogel to the ball milling beads is 1:

650.

3. The method for loading high-content platinum on carbon aerogel according to claim 1, characterized in that: In step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: sodium borohydride is dissolved in ultrapure water to prepare a sodium borohydride solution and poured into a separatory funnel for later use; chloroplatinic acid aqueous solution and the carbon aerogel powder obtained in step (5) are added to ultrapure water, and a precursor solution is formed after uniform dispersion by ultrasonication; the sodium borohydride solution is added dropwise to the precursor solution while stirring, and stirring is maintained for 10 to 15 hours after the addition is completed, and then the reaction solution is filtered, rinsed with ultrapure water, and the filter cake is dried in a vacuum environment at 60 to 80° C. for 10 to 15 hours to obtain a carbon aerogel-loaded platinum catalyst.

4. The method for loading high-content platinum on carbon aerogel according to claim 1, characterized in that: In step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: take the ball-milled carbon aerogel powder and place it in a culture dish, spread it evenly, drop chloroplatinic acid solution into it and ultrasonically disperse it evenly, and put it together with the culture dish into a UV curing furnace for UV reduction, so as to obtain a carbon aerogel-loaded platinum catalyst.

5. The method for loading high-content platinum on carbon aerogel according to claim 4, characterized in that: In the ultraviolet reduction operation, the illumination time was set to 85 minutes and the illumination power was set to 100%.

6. The method for loading high-content platinum on carbon aerogel according to claim 1, characterized in that: In step (6), the specific operation of loading platinum on the carbon aerogel powder is as follows: adding chloroplatinic acid solution to ethylene glycol, adjusting the pH to 13 with sodium hydroxide solution, and then adding ball-milled carbon aerogel powder, and forming a precursor solution after ultrasonic dispersion; pouring the precursor solution into a three-necked flask and carrying out an oil bath at 130° C. for 4 hours, cooling to room temperature and slowly adding concentrated acid dropwise until the pH is less than 3, maintaining stirring for 12 hours, then filtering the reaction solution, first rinsing with acetone and then rinsing with ultrapure water, and taking the filter cake and drying it in a vacuum environment at 60 to 80° C. for 10 to 15 hours to obtain a carbon aerogel-loaded platinum catalyst.