Poly(lactic acid-B-3-hydroxypropionic acid) block copolymers having excellent transparency properties and products containing the same

By controlling the degree of introduction of 3-hydroxypropionic acid monomer, poly(lactic acid-b-3-hydroxypropionic acid) block copolymers were prepared, which improved the transparency and mechanical properties of polylactic acid and solved the problem of the application limitations of polylactic acid.

CN115956096BActive Publication Date: 2024-11-22LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280005611.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2022-02-24
Publication Date
2024-11-22
Estimated Expiration
2042-02-24

AI Technical Summary

Technical Problem

Polylactic acid has poor impact resistance and heat resistance, insufficient transparency, and weak tensile strength, making it difficult to meet the needs of most applications.

Method used

Poly(lactic acid-b-3-hydroxypropionic acid) block copolymers were prepared by controlling the degree of introduction of 3-hydroxypropionic acid monomers, and their physical properties such as transparency, elongation and tensile strength were optimized.

Benefits of technology

This has enabled polylactic acid to achieve a transparency of over 80%, an elongation of 1% to 250%, and a tensile strength of 30 MPa to 60 MPa, thus expanding its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004918462270000011
    Figure FDA0004918462270000011
  • Figure GDA0004080313550000021
    Figure GDA0004080313550000021
  • Figure GDA0004080313550000071
    Figure GDA0004080313550000071
Patent Text Reader

Abstract

Provided is a poly(lactic acid-b-3-hydroxypropionic acid) block copolymer, wherein the transparency of the polylactic acid is improved by introducing a monomer derived from 3-hydroxypropionic acid into the polylactic acid, thereby expanding its application field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2021-0024929 filed on February 24, 2021, the disclosure of which is incorporated herein by reference in its entirety.

[0003] The present invention relates to a poly (lactic acid-b-3-hydroxypropionic acid) block copolymer having excellent transparency performance and a product containing the same. Background Art

[0004] Polylactic acid (PLA) is a plant-derived resin obtained from plants such as corn, and has attracted widespread attention as an excellent environmentally friendly material due to its biodegradable properties. Unlike the existing commonly used petroleum-based resins such as polystyrene resins, polyvinyl chloride resins, polyethylene, etc., polylactic acid has the functions of preventing the depletion of petroleum resources and inhibiting carbon dioxide emissions, so it can reduce environmental pollution, which is a disadvantage of petroleum-based plastic products. Since environmental pollution problems caused by waste plastics, etc. have become social problems, efforts are being made to expand the application range of polylactic acid to products using conventional plastics (petroleum-based resins), such as food packaging materials and containers, electronic product housings, etc.

[0005] However, compared with existing petroleum-based resins, polylactic acid has poor impact resistance and heat resistance, so it has a limited range of applications. In addition, polylactic acid has weak tensile strength and requires transparency depending on the application field. Since it is difficult to control the physical properties of polylactic acid, polylactic acid has limitations as a general-purpose resin.

[0006] In order to improve the above-mentioned shortcomings, the copolymers containing other repeating units in polylactic acid have been studied, and in particular, 3-hydroxypropionic acid has received attention as a comonomer. However, polylactic acid exhibits different physical properties according to the introduction degree of 3-hydroxypropionic acid. When the introduction degree of 3-hydroxypropionic acid is not controlled, it is understood that the inherent physical properties of polylactic acid deteriorate.

[0007] Therefore, the present invention aims to provide a block copolymer having excellent physical properties such as transparency, etc., while maintaining the inherent physical properties of polylactic acid by controlling the degree of introduction of a monomer derived from 3-hydroxypropionic acid. Summary of the invention

[0008] Technical issues

[0009] Provided are a copolymer having excellent physical properties such as transparency, etc. while maintaining the inherent properties of polylactic acid; and an article comprising the copolymer.

[0010] Technical Solution

[0011] In order to achieve the above object, a poly(lactic acid-b-3-hydroxypropionic acid) block copolymer represented by the following Chemical Formula 1 is provided, wherein the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a UV transparency of 80% or more:

[0012] [Chemical formula 1]

[0013]

[0014] In Chemical Formula 1,

[0015] m is an integer from 100 to 1000, and

[0016] n is an integer ranging from 500 to 4000.

[0017] As used herein, the term "poly(lactic acid-b-3-hydroxypropionic acid) block copolymer" is a block copolymer obtained by polymerizing monomers derived from lactide and monomers derived from 3-hydroxypropionic acid, as shown in Chemical Formula 1, which refers to a block copolymer in which various physical properties of polylactic acid are controlled by introducing monomers derived from 3-hydroxypropionic acid.

[0018] When the monomer from 3-hydroxypropionic acid is introduced as a comonomer of polylactic acid, various physical properties of polylactic acid can be improved, but the physical properties exhibited will be different depending on the degree of introduction. Therefore, in the present invention, the degree of introduction of the monomer from 3-hydroxypropionic acid can be controlled to control physical properties such as transparency, etc., while maintaining the inherent physical properties of polylactic acid.

[0019] Preferably, m is 120 to 350. m represents the number of repetitions from the 3-hydroxypropionic acid monomer. When the monomer from 3-hydroxypropionic acid is introduced within the above range, physical properties such as transparency can be controlled while maintaining the inherent physical properties of polylactic acid. More preferably, m is 130 or more, 140 or more, 150 or more, 160 or more, 170 or more, 180 or more, 190 or more, or 200 or more; and is 340 or less, 330 or less, 320 or less, 310 or less, or 300 or less.

[0020] Preferably, n is 1000 to 2500. n represents the number of repetitions of the monomer derived from lactide. More preferably, n is 1100 or more, 1200 or more, 1300 or more, 1400 or more, or 1500 or more; and is 2400 or less, 2300 or less, 2200 or less, 2100 or less, or 2000 or less.

[0021] In addition, in the present invention, the relative ratio of the monomers is important, and preferably, m / n is 0.05 to 0.20. Within the above m / n range, physical properties such as transparency can be controlled while maintaining the inherent physical properties of polylactic acid. More preferably, m / n is 0.06 or more, 0.07 or more, or 0.08 or more; and 0.19 or less, 0.18 or less, 0.17 or less, 0.16 or less, or 0.15 or less.

[0022] Preferably, the UV transparency of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, or 90%. In addition, the upper limit of UV transparency is theoretically 100%, for example, 99.5% or less, 99.0% or less, 98.5% or less, or 98.0% or less. The method for measuring UV transparency will be described in detail in the embodiments described later.

[0023] Preferably, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is 1% to 250%. Preferably, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is more than 40%, more than 50%, more than 60%, more than 70%, more than 80%, more than 90% or more than 100%. In addition, the elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably less than 240%, less than 230%, less than 220%, less than 210%, less than 200%, less than 150% or less than 120%. The method for measuring elongation will be described in detail in the embodiment described later.

[0024] The tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is 30MPa to 60MPa. The method for measuring tensile strength will be described in detail in the embodiment described later. Preferably, the tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is more than 31MPa, more than 32MPa, more than 33MPa, more than 34MPa or more than 35MPa. At the same time, when the numerical value is higher, the tensile strength is more excellent. However, when the numerical value is too high, the application field of copolymer can be restricted. From this point of view, the tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably less than 60MPa. More preferably, the tensile strength of poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is less than 55MPa, less than 50MPa, less than 45MPa or less than 40MPa.

[0025] Furthermore, the tensile modulus of the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is preferably 1.5 GPa to 2.5 GPa. The method of measuring the tensile modulus will be described in detail in the examples described later.

[0026] In addition, the weight average molecular weight of the poly (lactic acid -b-3-hydroxypropionic acid) block copolymer is preferably 50,000 to 350,000. More preferably, the weight average molecular weight of the poly (lactic acid -b-3-hydroxypropionic acid) block copolymer is 60,000 or more, 70,000 or more, 80,000 or more, 90,000 or more, or 100,000 or more; and 300,000 or less, 250,000 or less, 200,000 or less, or 150,000 or less.

[0027] Also provided is a method for preparing the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer, which comprises the step of polymerizing a 3-hydroxypropionic acid polymer, lactide and a catalyst.

[0028] The 3-hydroxypropionic acid polymer refers to a homopolymer of 3-hydroxypropionic acid, and a polymer prepared by controlling the degree of polymerization in consideration of the above-mentioned ranges of m and n is used.

[0029] Meanwhile, since the lactide ring-opening polymerization reaction is involved, the preparation method is carried out in the presence of a lactide ring-opening catalyst. For example, the catalyst may be a catalyst represented by Chemical Formula 2.

[0030] [Chemical formula 2]

[0031] MA 1 p A 2 2_p

[0032] In chemical formula 2,

[0033] M is Al, Mg, Zn, Ca, Sn, Fe, Y, Sm, Lu, Ti, or Zr,

[0034] p is an integer from 0 to 2, and

[0035] A 1 and A 2 Each is independently an alkoxy group or a carboxyl group.

[0036] More specifically, the catalyst represented by Chemical Formula 2 may be tin(II)-2-ethylhexanoate (Sn(O C t)2).

[0037] Preferably, when the total mole number of lactide is considered to be 100 mol %, the catalyst may be used in an amount of 0.001 mol % to 10 mol %, 0.01 mol % to 5 mol %, or 0.03 mol % to 1 mol %.

[0038] Preferably, the preparation method is carried out at a temperature of 150° C. to 200° C. Preferably, the preparation method is carried out for 5 minutes to 10 hours, and more preferably, for 10 minutes to 1 hour. Preferably, the preparation method is carried out at 0.5 atm to 1.5 atm.

[0039] Also provided is a product comprising the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer.

[0040] Beneficial Effects

[0041] As described above, the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to the present invention is characterized in that the transparency of polylactic acid is improved by introducing a monomer derived from 3-hydroxypropionic acid into polylactic acid, thereby expanding its application fields. DETAILED DESCRIPTION

[0042] Hereinafter, embodiments of the present invention will be described in more detail in the following examples. However, the following examples are only used to illustrate embodiments of the present invention, and the content of the present invention is not limited by the following examples.

[0043] Preparation Example: Preparation of poly (3-hydroxypropionate) oligomer

[0044] For the biosynthesis of high molecular weight poly (3-hydroxypropionate) according to the present invention, fermentation is first performed under the following conditions to prepare a fermentation broth containing 3-hydroxypropionate as a fermentation substrate. Specifically, Escherichia coli (E. coli) W3110 having GDH and ALDH enzyme genes is used as a fermentation strain. M9 is used as a culture medium, and 70 g / L of glycerol is used as a substrate for fermentation to produce 3-hydroxypropionate.

[0045] Afterwards, the prepared 3-hydroxypropionic acid ester was used as a substrate to produce poly-(3-hydroxypropionic acid) (hereinafter referred to as "P(3HP)") by fermentation. Specifically, a 5L fermentor (internal volume: 3L) was used for fermentation. As a fermentation microorganism, a recombinant Escherichia coli prepared by converting a recombinant vector into XL1-Blue Escherichia coli was used, wherein the recombinant vector was prepared by cloning the RecC gene as a polyhydroxyalkanoate synthase (PHA synthase) from Ralstonia eutropha and the propionyl-CoA transferase variant 540 (CPPCT_540) gene from Clostridium propionicum into a pBLuescript II KS+ vector.

[0046] The CPPCT_540 gene is an improved gene whose nucleotide sequence is substituted to cause valine to be changed to alanine at position 193 (V194A), and three silent mutations (T669C, A1125G, and T1158C) occur only by DNA substitution without any other amino acid changes (WO 09 / 022797).

[0047] As a culture medium, a fermentation broth (2.0 g / L) prepared by adding glucose (20 g / L) and the 3-hydroxypropionate prepared above as substrates to a modified Riesenberg (MR) medium was introduced. The fermentation broth was fermented by aeration at 300 rpm and 1 vvm to finally produce high molecular weight poly (3-hydroxypropionate) (Mn: 136,645; Mw: 354,615; PDI: 2.60; measured using an Agilent 1200 series and calibrated with a PC standard).

[0048] The prepared poly(3-hydroxypropionate) was placed in distilled water and hydrolyzed at 100°C for 12 hours, 18 hours, 24 hours, and 72 hours, respectively, to obtain poly(3-hydroxypropionate) oligomers with weight average molecular weights of 15,000 g / mol, 30,000 g / mol, 60,000 g / mol, and 80,000 g / mol, respectively (measured using Agilent 1200 series and calibrated by PC standards).

[0049] Example 1: Preparation of poly(lactic acid-b-3-hydroxypropionic acid) block copolymer

[0050] Add lactide (25g), poly (3-hydroxypropionate) oligomer (3g) with a weight average molecular weight of 15,000g / mol prepared in the above preparation example, ethylhexanoate tin (II) (0.014g) and toluene (100uL) as a catalyst in the reactor, and then dry for about 30 minutes to about 1 hour. Then, the reactor is placed in an oil bath preheated to 180°C and polymerized for 1.5 hours. After taking out the product from the reactor, the product is devolatilized at 140°C and 1 to 5 torr under reduced pressure for about 3 hours to remove the monomer. Finally, a poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is prepared.

[0051] Examples 2 to 5 and Comparative Examples: Preparation of poly(lactic acid-b-3-hydroxypropionic acid) block copolymers

[0052] Each poly(lactic acid-b-3-hydroxypropionic acid) block copolymer was prepared in the same manner as in Example 1, except that the raw materials were changed as shown in Table 1 below.

[0053] [Table 1]

[0054]

[0055]

[0056] Test example

[0057] The properties of the copolymers prepared in the examples were evaluated as follows.

[0058] - Weight average molecular weight: measured by GPC using Agilent 1200 series and PC standard.

[0059] - Elongation, tensile strength and tensile modulus: performed according to ASTM D638. ASTM D536 V-type specimens were manufactured using a hot press device (Limotem QM900S) and then measured using a universal testing machine (UTM) at a load of 10 mm / s and 60 kg / f.

[0060] - Content of 3-hydroxypropionic acid in the block copolymer (wt%): measured by NMR analysis of the block copolymer.

[0061] - UV transparency: The copolymer was prepared into a 80 um thick sheet using a heat press device (Limotem QM900S), and then attached to a UV-visible spectrometer (Agilent 8453) to measure transparency. At this time, the transparency value at 480 nm region was detected.

[0062] The measurement results are shown in the following table.

[0063] [Table 2]

[0064]

Claims

1. A poly (lactic acid-b-3-hydroxypropionic acid) block copolymer represented by the following chemical formula 1, in, The UV transparency of the poly(lactic acid-b-3-hydroxypropionic acid) block copolymer is above 80%: [Chemical formula 1] In Chemical Formula 1, m is an integer from 120 to 350, and n is an integer from 500 to 4000, and Wherein, m / n is 0.05 to 0.

20.

2. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, n is from 1000 to 2500.

3. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, The elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is 1% to 250%.

4. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, The elongation of the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer is 5% to 35%.

5. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a tensile strength of 30 MPa to 60 MPa.

6. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a tensile modulus of 1.5 GPa to 2.5 GPa.

7. The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer according to claim 1, in, The poly(lactic acid-b-3-hydroxypropionic acid) block copolymer has a weight average molecular weight of 50,000 to 350,000.

8. An article comprising the poly (lactic acid-b-3-hydroxypropionic acid) block copolymer according to any one of claims 1 to 7.