Production method of hydrophilic light nano calcium carbonate

By using triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants in the reaction of calcium hydroxide slurry and carbonized gas, and controlling the reaction conditions, the problems of hydrophobicity, poor dispersion and easy agglomeration of nano-calcium were solved , generating hydrophilic lightweight nano-calcium carbonate, realizing its wide application in polymer materials and environmentally friendly degradation properties.

CN115959697BActive Publication Date: 2024-10-29GUANGXI LAIBIN GUOHONG CALCIUM TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310054760.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-03
Publication Date
2024-10-29
Estimated Expiration
2043-02-03

AI Technical Summary

Technical Problem

The nano-calcium produced by the existing technology has hydrophobicity, poor dispersion, low adhesion, easy agglomeration and poor whiteness, which limits its application in coatings and polymer materials, and is especially difficult to degrade in environmentally friendly degradable materials.

Method used

Calcium hydroxide slurry and carbonized gas are used to carry out carbonization reaction with triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants. The reaction conditions such as pressure and temperature are controlled, and a crystal stabilizer is added to generate a hydrophilic light Quality nano calcium carbonate.

Benefits of technology

The obtained nano-calcium carbonate is hydrophilic, easy to depolymerize, degradable and has high whiteness. It is suitable for adding and modifying water-soluble and water-insoluble polymer materials, simplifying the process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115959697B_ABST
    Figure CN115959697B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano material preparation, and proposes a method for producing hydrophilic light nano calcium carbonate, wherein calcium hydroxide slurry and carbonized gas are subjected to carbonization reaction under triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants to synthesize nano calcium carbonate. Through the above technical scheme, the problems that the nano calcium carbonate produced in the prior art has poor dispersibility and low adhesion due to hydrophobicity, and is prone to precipitation, easy agglomeration, and poor whiteness when applied to coating production are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano material preparation, and in particular to a method for producing hydrophilic light nano calcium carbonate. Background Art

[0002] The invention and industrial application of nano-scale light calcium carbonate (hereinafter referred to as nano-calcium) have most significantly promoted the rapid development of the modern organic polymer new material industry. That is, as an additive for organic polymer materials, it will significantly change the physical and chemical properties of organic polymer materials. After adding an appropriate amount of nano-calcium, the applicability of organic polymer materials is greatly enhanced. After adding nano-calcium, the physical and chemical properties of materials such as rubber, plastics, coatings, inks, paper, sealing coatings, thermal insulation, etc. have been fully changed and show excellent applicability.

[0003] The main process of producing nano calcium in the prior art is: limestone is decomposed into calcium oxide and carbon dioxide gas by calcination, calcium oxide is converted into calcium hydroxide slurry by hydrolysis, and calcium hydroxide slurry is carbonized with carbon dioxide gas under certain conditions to generate nano calcium. The contact reaction of calcium hydroxide and carbon dioxide gas is the key process of generating nano calcium in these processes. And nano calcium has strong agglomeration and certain chemical polarity due to its small particle size. For this reason, the prior art is to add dispersant and surfactant respectively during and after the reaction to coat the calcium carbonate crystal molecular group, so as to improve its processability and be easy to non-polar chemical chelation, which plays an important role in generating nano calcium and being used as a polymer material filler.

[0004] The commonly used dispersants and surfactants are polyphosphates, sucrose and stearic acid complex salts. The defects of this process condition are:

[0005] (1) The produced nano calcium is coated with non-polar large molecular weight stearic acid hydrocarbon groups, which makes it hydrophobic, showing poor dispersibility and low adhesion, and is prone to precipitation when used in coating production. This makes it difficult to apply nano calcium in water-soluble coating materials, limiting the application projects of nano calcium.

[0006] (2) Nano calcium added with stearic acid complex salts is difficult to degrade after chelating with organic polymer materials, which is contrary to the requirements of environmentally friendly degradable materials. For example, nano calcium is required to have excellent degradability when added to polymer materials such as mulching, food packaging, and medical applications.

[0007] (3) Nano-calcium coated with stearic acid composite salt is easy to agglomerate and has poor whiteness, which makes depolymerization difficult and increases power consumption.

[0008] Therefore, those skilled in the art are committed to studying a process for producing hydrophilic, degradable, easily depolymerized, and high-whiteness nano calcium carbonate. Summary of the invention

[0009] The present invention provides a method for producing hydrophilic light nano-calcium carbonate, which solves the problems that the nano-calcium carbonate produced in the related art has hydrophobicity, resulting in poor dispersibility and low adhesion, and is prone to precipitation, easy agglomeration and poor whiteness when used in coating production.

[0010] The technical solution of the present invention is as follows:

[0011] The invention discloses a method for producing hydrophilic light nano calcium carbonate, wherein calcium hydroxide slurry and carbonization gas are subjected to carbonization reaction in the presence of triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants to synthesize nano calcium carbonate.

[0012] As a further technical solution, the mass concentration of the calcium hydroxide slurry is 8-10%.

[0013] As a further technical solution, the carbonized gas is lime kiln gas containing 35-40% carbon dioxide by volume.

[0014] As a further technical solution, the added amount of the dispersant is 3-5‰ of the dry weight of calcium carbonate.

[0015] As a further technical solution, the mass ratio of triethanolamine to N-(3-aminopropyl)diethanolamine in the dispersant is 3 to 5:1.

[0016] As a further technical solution, the carbonization reaction has a pressure of 40-60 kPa and a temperature of 20-25°C.

[0017] As a further technical solution, the carbonization reaction obtains nano-calcium carbonate cooked slurry, and the nano-calcium carbonate cooked slurry is centrifugally dehydrated, dried, and crushed to obtain nano-calcium carbonate.

[0018] As a further technical solution, the sign that the carbonization reaction is completed is that the pH value of the nano-calcium carbonate cooked slurry is 8-9.

[0019] As a further technical solution, the method for producing the hydrophilic light nano-calcium carbonate further comprises a crystal stabilizer, wherein the amount of the crystal stabilizer added is 0.4-1% of the dry weight of the calcium carbonate.

[0020] As a further technical solution, the crystal stabilizer includes one or more of polyacrylic acid, polyacrylamide, and polyaspartic acid.

[0021] The working principle and beneficial effects of the present invention are:

[0022] 1. The present invention provides a method for producing hydrophilic light nano-calcium carbonate, wherein the concentrations of the reactants are 8-10% by mass of calcium hydroxide slurry, the carbonized gas is lime kiln gas containing 35-40% by volume of carbon dioxide, and triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 3-5:1 are used as dispersants for the nano-calcium carbonate generation reaction and as a coating agent for the nano-calcium carbonate, and the added amount is 3-5‰ of the dry weight of the finished calcium carbonate, the reaction pressure is controlled at 40-60 kPa, and the reaction temperature is controlled at 20-25°C. The produced nano-calcium carbonate has the advantages of hydrophilicity, easy depolymerization, degradability, high whiteness, safety, environmental protection, and simple process.

[0023] 2. The surface of the nano calcium carbonate crystal molecular pellets or rhombohedral bodies obtained by the production method provided by the present invention is coated with trihydroxyl and dihydroxyl groups with strong polarity, so that it is easy to have affinity with water molecules with strong polarity and has hydrophilicity; at the same time, it also has functional groups that chelate with non-polar organic polymer materials, so that the nano calcium carbonate product has easy depolymerization and the added polymer material has easy degradation characteristics.

[0024] 3. The essence of the carbonization reaction is that CO2 combines with water molecules and ionizes into acid radical ions of different valences, and Ca(OH)2 ionizes into Ca 2+ and OH - After the ions, the two types of ions are subjected to different stages of neutralization precipitation reactions in the aqueous solution, and finally precipitated calcium carbonate is obtained, which is presented in the form of calcium carbonate molecular crystals, and the outer diameter of the generated calcium carbonate single crystal is about 60-120nm, which is called nano-scale light calcium carbonate. The present invention adopts triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants and coating agents, coupled with a crystal stabilizer and a perfect reaction condition setting, and has the characteristics of simple operation, easy availability of raw materials, and relatively low cost. In addition, the hydrophilic nano calcium carbonate produced by the present invention has both hydrophilicity and non-polar molecular coupling, is easy to decompose, degradable, and has high whiteness, and can be widely used in the filling and modification of water-soluble and non-water-soluble organic polymer materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0026] Figure 1 This is a scanning electron microscope image of the crystal morphology of nano calcium carbonate obtained in Example 1 of the present invention, magnified 5,000 times and with a scale of 1 micron;

[0027] Figure 2 This is a scanning electron microscope image of the crystal morphology of nano calcium carbonate obtained in Example 1 of the present invention, magnified 10,000 times with a scale of 500 nanometers;

[0028] Figure 3This is a scanning electron microscope image of the crystal morphology of nano calcium carbonate obtained in Example 1 of the present invention, magnified 20,000 times with a scale of 200 nanometers;

[0029] Figure 4 This is a scanning electron microscope image of the crystal morphology of nano-calcium carbonate obtained in Example 1 of the present invention, magnified 35,000 times and with a scale of 100 nanometers. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] The mass concentration of the calcium hydroxide slurry is adjusted to 9%, and the temperature is adjusted to 23° C., and the slurry is delivered to the carbonization kettle by a centrifugal pump. When the slurry level in the kettle reaches the requirement, the delivery is stopped, the stirring is started, the solid content in the kettle is calculated and converted into the dry basis amount of the finished calcium carbonate, and a dispersant of 4‰ of the dry basis weight of the calcium carbonate is added by a metering pump, the temperature in the kettle is controlled at 23° C. by circulating cooling water, 0.5% of the dry basis weight of the calcium carbonate is added, and lime kiln gas containing 38% CO2 is continuously introduced into the kettle at a pressure of 50 kPa and a stable airflow to obtain a nano calcium carbonate cooked slurry, wherein the dispersant is composed of triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 4:1;

[0033] When the pH of the cooked nano-calcium carbonate slurry is 8, the reaction is completed, and nano-calcium carbonate is obtained after centrifugal dehydration, drying and crushing.

[0034] Example 2

[0035] The mass concentration of calcium hydroxide slurry is adjusted to 8%, and the temperature is adjusted to 20°C, and the slurry is delivered to the carbonization kettle by a centrifugal pump. When the slurry level in the kettle reaches the requirement, the delivery is stopped, the stirring is started, the solid content in the kettle is calculated and converted into the dry basis amount of finished calcium carbonate, and a dispersant of 3‰ of the dry basis weight of calcium carbonate is added by a metering pump, the temperature in the kettle is controlled at 20°C by circulating cooling water, polyacrylamide of 0.4% of the dry basis weight of calcium carbonate is added, and lime kiln gas containing 35% CO2 is continuously introduced into the kettle at a pressure of 40kPa and a stable airflow to obtain a nano calcium carbonate cooked slurry, wherein the dispersant is composed of triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 3:1;

[0036] When the pH of the nano calcium carbonate cooked slurry is 8.5, the reaction is completed, and nano calcium carbonate is obtained after centrifugal dehydration, drying and crushing.

[0037] Example 3

[0038] The mass concentration of calcium hydroxide slurry is adjusted to 10%, and the temperature is adjusted to 25°C, and the slurry is delivered to the carbonization kettle by a centrifugal pump. When the slurry level in the kettle reaches the requirement, the delivery is stopped, the stirring is started, the solid content in the kettle is calculated and converted into the dry basis amount of finished calcium carbonate, and a dispersant of 5‰ of the dry basis weight of calcium carbonate is added by a metering pump, the temperature in the kettle is controlled at 25°C by circulating cooling water, 1% of polyaspartic acid of the dry basis weight of calcium carbonate is added, and lime kiln gas containing 40% CO2 is continuously introduced into the kettle at a pressure of 60kPa and a stable airflow to obtain a nano calcium carbonate cooked slurry, wherein the dispersant is composed of triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 5:1;

[0039] When the pH of the nano calcium carbonate cooked slurry is 9, the reaction is completed, and nano calcium carbonate is obtained after centrifugal dehydration, drying and crushing.

[0040] Example 4

[0041] The mass concentration of the calcium hydroxide slurry is adjusted to 9%, and the temperature is adjusted to 23° C., and the slurry is delivered to the carbonization kettle by a centrifugal pump. When the slurry level in the kettle reaches the requirement, the delivery is stopped, the stirring is started, the solid content in the kettle is calculated and converted into the dry basis amount of the finished calcium carbonate, and a dispersant of 4‰ of the dry basis weight of the calcium carbonate is added by a metering pump, the temperature in the kettle is controlled at 23° C. by circulating cooling water, 0.5% of the dry basis weight of the calcium carbonate is added, and lime kiln gas containing 38% CO2 is continuously introduced into the kettle at a pressure of 50 kPa and a stable airflow to obtain a nano calcium carbonate cooked slurry, wherein the dispersant is composed of triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 4:1;

[0042] When the pH of the nano calcium carbonate cooked slurry is 7.5, the reaction is completed, and nano calcium carbonate is obtained after centrifugal dehydration, drying and crushing.

[0043] Example 5

[0044] The mass concentration of the calcium hydroxide slurry is adjusted to 9%, and the temperature is adjusted to 23° C., and the slurry is delivered to the carbonization kettle by a centrifugal pump. When the slurry level in the kettle reaches the requirement, the delivery is stopped, the stirring is started, the solid content in the kettle is calculated and converted into the dry basis amount of the finished calcium carbonate, and a dispersant of 1% by weight of the dry basis of the calcium carbonate is added by a metering pump, the temperature in the kettle is controlled at 23° C. by circulating cooling water, and 0.5% by weight of polyacrylic acid of the dry basis of the calcium carbonate is added, and lime kiln gas containing 38% CO2 is continuously introduced into the kettle at a pressure of 50 kPa and a stable airflow to obtain a cooked nano calcium carbonate slurry, wherein the dispersant is composed of triethanolamine and N-(3-aminopropyl)diethanolamine in a mass ratio of 4:1;

[0045] When the pH of the cooked nano-calcium carbonate slurry is 8, the reaction is completed, and nano-calcium carbonate is obtained after centrifugal dehydration, drying and crushing.

[0046] Comparative Example 1

[0047] The only difference from Example 1 is that the dispersant is triethanolamine.

[0048] Comparative Example 2

[0049] The only difference from Example 1 is that the dispersant is N-(3-aminopropyl)diethanolamine.

[0050] Comparative Example 3

[0051] The only difference from Example 1 is that no dispersant is added.

[0052] The nano calcium carbonate obtained in Examples 1 to 5 and Comparative Examples 1 to 3 was tested for whiteness with reference to GB / T 19281-2014, and the test results are recorded in Table 1.

[0053] Table 1 Whiteness of nano calcium carbonate

[0054] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Comparative Example 3 Whiteness / % 97.2 96.1 96.8 95.3 95.5 94.9 94.4 92.6

[0055] As can be seen from Table 1, the nano calcium carbonate obtained by the production method of hydrophilic light nano calcium carbonate provided by the present invention has a whiteness of more than 95.3%. In Comparative Example 1, the dispersant is triethanolamine, in Comparative Example 2, the dispersant is N-(3-aminopropyl)diethanolamine, and in Comparative Example 3, no dispersant is added. The whiteness of the nano calcium carbonate obtained in Comparative Examples 1 to 3 is lower than that in the embodiment. Therefore, when triethanolamine and N-(3-aminopropyl)diethanolamine are used as dispersants, the whiteness of the nano calcium carbonate obtained is the best.

[0056] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing hydrophilic light nano calcium carbonate, characterized in that: The calcium hydroxide slurry and carbonization gas are subjected to carbonization reaction in the presence of triethanolamine and N-(3-aminopropyl)diethanolamine as dispersants to synthesize nano calcium carbonate. The amount of dispersant added is 3~5‰ of the dry weight of calcium carbonate; The mass ratio of triethanolamine to N-(3-aminopropyl)diethanolamine in the dispersant is 3-5:1; The carbonized gas is lime kiln gas containing 35-40% carbon dioxide by volume.

2. The production method of hydrophilic light nano calcium carbonate according to claim 1, characterized in that, The mass concentration of the calcium hydroxide slurry is 8-10%.

3. The production method of hydrophilic light nano calcium carbonate according to claim 1, characterized in that, The carbonization reaction has a pressure of 40-60 kPa and a temperature of 20-25°C.

4. The production method of hydrophilic light nano calcium carbonate according to claim 1, characterized in that: The carbonization reaction obtains nano-calcium carbonate cooked slurry, and the nano-calcium carbonate cooked slurry is centrifugally dehydrated, dried, and crushed to obtain nano-calcium carbonate.

5. The production method of hydrophilic light nano calcium carbonate according to claim 4, characterized in that, The sign of completion of the carbonization reaction is that the pH value of the nano calcium carbonate cooked slurry is 8-9.

6. The production method of hydrophilic light nano calcium carbonate according to claim 1, characterized in that: It also includes a crystal stabilizer, and the added amount of the crystal stabilizer is 0.4-1% of the dry weight of calcium carbonate.

7. The production method of hydrophilic light nano calcium carbonate according to claim 6, characterized in that: The crystal stabilizer includes one or more of polyacrylic acid, polyacrylamide and polyaspartic acid.

Citation Information

Patent Citations

  • Preparation method of nano calcium carbonate capable of stably suspending and dispersing in aqueous solution

    CN109879303A

  • Industrial process for preparing nm-class active calcium carbonate

    CN1330039A