A kind of high purity beta gallium oxide nano microsphere and preparation method thereof

Through hydrothermal reaction and atomized plasma spheroidization technology, high-purity and high spherical β gallium oxide nano microspheres were prepared, which solved the problem of insufficient fluidity and dispersion of gallium oxide particles in the prior art, and achieved high Purity and excellent fluidity, suitable for film preparation.

CN115974133BActive Publication Date: 2024-11-22ZHUZHOU KENENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211673360.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-22
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

It is difficult to prepare high-purity β-gallium oxide nano-microspheres in the prior art, and the gallium oxide particles cannot meet the requirements of fluidity and dispersion, affecting the quality and stability of the film.

Method used

By reacting metal Ga with ultrapure water with hydrothermal, adjusting the solid-liquid ratio and atomizing, the plasma spheroidization technology is used to convert hydroxyl gallium oxide into β gallium oxide at high temperature to form spherical micropowder to control the atomized gas medium Pressure and plasma power to ensure spheroidization and dispersion.

Benefits of technology

Beta gallium oxide nano microspheres with high purity (≥5N), high spherical shape and narrow particle size distribution were prepared, which had excellent fluidity and dispersion, simplified the process and were suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974133B_ABST
    Figure CN115974133B_ABST
Patent Text Reader

Abstract

The invention discloses a high-purity β-gallium oxide nano-microsphere and a preparation method thereof. Metal Ga is mixed with ultrapure water to obtain a mixed liquid, which is subjected to hydrothermal reaction to obtain a gallium oxide hydroxyl precipitate suspension A. The solid-liquid ratio of the gallium oxide hydroxyl precipitate suspension A is adjusted to obtain a gallium oxide hydroxyl precipitate suspension B. The gallium oxide hydroxyl precipitate suspension B is transported to an atomizing nozzle under continuous stirring, and is atomized into droplets by an atomizing gas medium, and the droplets are spheroidized by plasma to obtain the high-purity β-gallium oxide nano-microsphere. The high-purity β-gallium oxide nano-microsphere obtained by the preparation method provided by the invention has a purity of ≥5N, a narrow particle size distribution, a high sphericity, and excellent fluidity and dispersibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to high-purity beta-gallium oxide nano-microspheres and a preparation method thereof, belonging to the technical field of semiconductor material preparation. Background Art

[0002] Gallium oxide (Ga2O3) is an important wide bandgap semiconductor material. It has five crystal structures: α-Ga2O3, β-Ga2O3, γ-Ga2O3, ε-Ga2O3 and δ-Ga2O3, which can transform into each other under certain conditions. Among them, β-Ga2O3 is the most stable, with a monoclinic structure at room temperature and a spatial structure of C2 / m. β=103.83°. Ga2O3 has excellent photoluminescence properties, chemical and thermal stability, and is widely used in sensitive materials, catalysts, optoelectronic materials, phosphors, and other fields.

[0003] In recent years, the application of IGZO (indium gallium zinc oxide) in the field of TFT-LCD displays has reduced the number of transistors, improved the transmittance of each pixel, and made the display have a higher energy efficiency level and higher efficiency. At present, the radio frequency / direct current (RF / DC) sputtering system is the mainstream thin film growth equipment. In addition to the thin film deposition process, the factors affecting the quality of sputtered transparent conductive films include the density, conductivity, grain size, microstructure and purity of the target material. For example, if the density of the target material is low, that is, there are micropores on the surface or inside the target material, the coating process will cause protrusions on the surface of the target material, causing the local energy of the target material to be too high, and the oxygen ions are impacted into a free state, forming a high resistance area, causing some microparticles to enter the film, reducing the quality of the film, and thus affecting the stability of the coating.

[0004] At present, the IGZO sputtering targets sold in the commercial market are mainly sintered by solid phase reaction hot pressing. The method is to mix In2O3, ZnO and Ga2O3 powders in a certain proportion, ball mill homogenize, hot press sinter and other steps to make IGZO targets for sputtering. This preparation method is simple to operate, but the uniformity of mechanical ball milling mixing is affected by the particle size and morphology of each powder. The particle size, morphology, fluidity and dispersibility of In2O3, ZnO and Ga2O3 powders play a decisive role in the homogenization effect and hot pressing process.

[0005] Chinese patent application CN107010654B discloses a method for preparing a monodisperse gallium oxide powder and a high-density ceramic target. The invention uses more than 99.99% of metal gallium to dissolve in acid, then adds ammonia water for precipitation and aging to obtain a white precipitate, and then washes, filters, dries, calcines and other processes to obtain the product. However, the calcination temperature of this method is high, the microscopic particles of the obtained product are easy to agglomerate, and the uniformity of the product is reduced.

[0006] Chinese patent application CN106744730A discloses a two-step method for preparing gallium oxide and gallium nitride nanopowders using metallic gallium as a raw material, wherein metallic Ga and water are reacted at a mass ratio of 1:2 to 10 in a high pressure reactor at 180-280°C to obtain gallium oxyhydroxide, and then the gallium oxyhydroxide is heated and decomposed in air at a temperature of 400°C to 800°C to obtain gallium oxide nanopowder with a particle size of 10-20nm.

[0007] However, the above-mentioned prior art does not produce spherical nano-scale gallium oxide particles, and the obtained gallium oxide particles cannot meet the requirements of fluidity and dispersibility. Summary of the invention

[0008] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing high-purity β-gallium oxide nanoparticles.

[0009] The second object of the present invention is to provide high-purity β-gallium oxide nano-microspheres prepared by the above preparation method.

[0010] In order to achieve the above object, the present invention adopts the following technical solution:

[0011] The invention discloses a method for preparing high-purity beta gallium oxide nano-microspheres. The method comprises the following steps: mixing metal Ga with ultrapure water to obtain a mixed solution, performing a hydrothermal reaction on the mixed solution, obtaining a gallium oxide hydroxyl precipitate suspension A, adjusting the solid-liquid ratio of the gallium oxide hydroxyl precipitate suspension A, obtaining a gallium oxide hydroxyl precipitate suspension B, conveying the gallium oxide hydroxyl precipitate suspension B to an atomizing nozzle under continuous stirring, atomizing the atomizing gas medium into droplets, and subjecting the droplets to plasma spheroidization to obtain the high-purity beta gallium oxide nano-microspheres.

[0012] The preparation method provided by the present invention comprises the following steps: firstly subjecting metal Ga and ultrapure water to a hydrothermal reaction to obtain a gallium oxyhydroxide precipitation suspension A, adjusting the solid-liquid ratio, and then atomizing the suspension to obtain small droplets, which are then fed into a plasma flame flow for high-temperature spray pyrolysis. The water in the suspension droplets can be rapidly volatilized under an ultra-high temperature and high-speed environment, and the gallium oxyhydroxide is pyrolyzed at a high temperature to become β-gallium oxide, which is melted on the surface under the action of the high temperature of the plasma, and spherical droplets are formed due to the action of surface tension, and spherical micropowders are formed after cooling.

[0013] In a preferred embodiment, the purity of the metal Ga is ≥5N.

[0014] Preferably, the resistivity of the ultrapure water is not less than 18 MΩ.cm (25° C.).

[0015] In the present invention, to obtain β-gallium oxide nano-microspheres with a purity of 5N or above, it is first necessary to ensure that the purity of the raw material metal gallium is not less than 5N and the resistivity of pure water is not less than 18MΩ.cm (25°C).

[0016] In a preferred embodiment, the mass ratio of the metal Ga to ultrapure water is 1:2-10.

[0017] In a preferred embodiment, the temperature of the hydrothermal reaction is 180-280° C., and the time of the hydrothermal reaction is 5-8 hours.

[0018] In the actual operation process, metallic Ga is mixed with ultrapure water and placed in a high-pressure reactor for reaction.

[0019] In a preferred embodiment, in the gallium oxyhydroxide precipitate suspension B, the mass ratio of the gallium oxyhydroxide precipitate to water is 10-15:90-85.

[0020] The inventors have found that it is crucial to control the solid-liquid mass ratio of gallium oxyhydroxide precipitate to water in the gallium oxyhydroxide precipitate suspension B within the above range. If there is too much liquid phase, the spheroidization efficiency will be low and the preparation amount will be small; if there is too little liquid phase, the spheroidization ratio will be low, and some gallium oxyhydroxide will be converted into β--Ga2O3 without forming spheres.

[0021] In the actual operation process, the gallium oxyhydroxide precipitation suspension B is continuously stirred while being transported to the atomizing nozzle by a DC pump.

[0022] In a preferred embodiment, the atomizing gas medium is selected from argon with a purity of ≥5N.

[0023] Preferably, the pressure of the atomizing gas medium is 1.6-2.2 MPa.

[0024] The inventors have found that when the pressure of the atomizing gas medium is controlled within the above range, the final spheroidization rate is the highest. If the atomizing pressure is small, the gallium oxyhydroxide suspension is not fully atomized. Excessive pressure will affect the stability of the plasma flame. Only a stable DC plasma flame can ensure the stable decomposition and spheroidization of the atomized gallium oxyhydroxide. Therefore, if the pressure of the atomizing gas medium is too high or too low, it will affect the final spheroidization effect.

[0025] In a preferred embodiment, the flow rate of the atomizing gas medium is 0.5 L / min to 2.5 L / min.

[0026] In a preferred embodiment, when the plasma is spheroidized, the power of the plasma is 9.75 KW to 12.8 KW.

[0027] The inventors have found that when the power of plasma spheroidization is controlled within the above range, the spheroidization rate is high and the dispersibility is good. If the power is too low, the gallium oxyhydroxide spheroidization rate is low, and if the power is too high, gallium oxyhydroxide may be converted into β-gallium oxide and melted and agglomerated.

[0028] The present invention also provides a high-purity beta-gallium oxide nano-microsphere prepared by the preparation method.

[0029] The purity of the high-purity beta-gallium oxide nano-microspheres is ≥5N, and the particle size of the high-purity beta-gallium oxide nano-microspheres is 100-500nm.

[0030] Principles and advantages

[0031] The invention provides a preparation method of high-purity beta-gallium oxide nano-microspheres. The method comprises the following steps: firstly, metal Ga and ultrapure water are subjected to hydrothermal reaction to obtain gallium oxide hydroxide precipitation suspension A, and after adjusting the solid-liquid ratio, atomization is performed to obtain small droplets, which are sent into a plasma flame flow for high-temperature spray pyrolysis. The water content of the suspension droplets can be rapidly volatilized under an ultra-high temperature and high-speed environment. The gallium oxide hydroxide is pyrolyzed at high temperature to become beta-gallium oxide, and the surface is melted under the action of plasma high temperature. Spherical droplets are formed due to the action of surface tension, and spherical micropowder is formed after cooling. The high-purity beta-gallium oxide nano-microspheres prepared by the preparation method provided by the invention have a purity of ≥5N, a narrow particle size distribution, a high sphericity, and excellent fluidity and dispersibility.

[0032] The present invention provides a novel method for preparing high-purity gallium oxide nano-microspheres, which can overcome the defects of gallium oxide prepared by the current process, such as large grain size, complex process and difficult process control. The process is simple and is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a scanning electron microscope photograph of the high-purity β-gallium oxide spherical powder obtained in Example 1.

[0034] Figure 2 This is a scanning electron microscope photograph of the high-purity β-gallium oxide spherical powder obtained in Example 2.

[0035] Figure 3 This is a scanning electron microscope photograph of the high-purity β-gallium oxide spherical powder obtained in Comparative Example 1. DETAILED DESCRIPTION

[0036] The present invention and its specific implementation methods are further described in detail below with reference to the embodiments.

[0037] The present invention is characterized by the following steps:

[0038] A. 5N metal Ga and ultrapure water with a resistivity of not less than 18 MΩ.cm (25° C.) are reacted in a high pressure reactor at a mass ratio of 1:2-10 at 180-280° C. to obtain a gallium oxyhydroxide precipitation suspension.

[0039] B. Adjust the mass ratio of the gallium oxyhydroxide precipitate suspension obtained in step A to between 10-15:90-85, convey it to the atomizing nozzle with a DC pump while stirring continuously, and atomize it with 5N argon gas with a pressure of 1.6-2.2 MPa and a flow rate of 0.5 L / min-2.5 L / min to form droplets with the smallest possible particle size.

[0040] C. The atomized droplets obtained in step B are fed into a plasma flame flow for high-temperature spray pyrolysis. The plasma power is controlled to be 9.75KW to 12.8KW. The water in the suspended droplets can be rapidly volatilized under an ultra-high temperature and high-speed environment. Gallium oxyhydroxide is pyrolyzed into gallium oxide, and melted on the surface under the action of the high temperature of the plasma. Spherical droplets are formed due to the action of surface tension, and spherical micropowders are formed after cooling.

[0041] The raw materials of the gallium oxyhydroxide precipitation suspension are 5N metal gallium and ultrapure water with a resistivity not less than 18MΩ.cm (25°C).

[0042] Embodiments of the present invention are given below:

[0043] Example 1

[0044] 10 grams of metal gallium and 50 grams of water are reacted in a high-pressure reactor at a reaction temperature of 250°C for a reaction time of 5 hours to obtain a gallium oxyhydroxide precipitation suspension. The solid-liquid mass ratio in the gallium oxyhydroxide precipitation suspension is adjusted to 10:90, and the suspension is continuously stirred while being transported to an atomizing nozzle using a DC pump, and atomized using 5N argon gas at a pressure of 1.6 MPa to form droplets with a particle size as small as possible. The droplets obtained after atomization are sent to a plasma flame flow with a power of 9.75KW for high-temperature spray pyrolysis, and spherical gallium oxide micropowders are formed after cooling. Figure 1 This is a scanning electron microscope photo of the high-purity β-gallium oxide spherical powder obtained in Example 1, from which it can be found that the sphericity rate is high, the particle size D50 is 220nm, and the purity is ≥99.999%. The impurity content detection results are shown in Table 1.

[0045] Example 2

[0046] 20 grams of metal gallium and 150 grams of water are reacted in a high-pressure reactor at a reaction temperature of 250°C for a reaction time of 5 hours to obtain a gallium oxyhydroxide precipitation suspension. The solid-liquid mass ratio in the gallium oxyhydroxide precipitation suspension is adjusted to 15:85, and the suspension is continuously stirred while being transported to an atomizing nozzle using a DC pump, and atomized using 5N argon gas at a pressure of 2.2 MPa to form droplets with a particle size as small as possible. The droplets obtained after atomization are sent to a plasma flame flow with a power of 12.8KW for high-temperature spray pyrolysis, and spherical gallium oxide micropowders are formed after cooling. Figure 2 This is a scanning electron microscope photo of the high-purity β-gallium oxide spherical powder obtained in Example 2, with a particle size D50 of 490 nm and a purity of ≥99.999%. The impurity content test results are shown in Table 1.

[0047] Comparative Example 1

[0048] The other conditions were the same as those in Example 2. The 5N argon gas with a pressure of 1.8 MPa was used to atomize the particles to form droplets with a particle size as small as possible. The droplets obtained after atomization were sent to a plasma flame with a power of 19.5 KW for high-temperature spray pyrolysis, and after cooling, they were agglomerated into large spherical gallium oxide micropowders. Figure 3 This is a scanning electron microscope photo of the high-purity β-gallium oxide spherical micropowder of comparative example 3, from which it can be found that due to the excessively high plasma power, gallium oxyhydroxide is converted into β-gallium oxide and then melted and agglomerated, resulting in a larger micropowder particle size, with D50 reaching 35 μm. The impurity content detection results are shown in Table 1.

[0049] Table 1

[0050]

Claims

1. A method for preparing high-purity β-gallium oxide nanospheres, characterized in that: The metal Ga and ultrapure water are mixed to obtain a mixed solution, which is subjected to a hydrothermal reaction to obtain a gallium oxyhydroxide precipitate suspension A, and the solid-liquid ratio of the gallium oxyhydroxide precipitate suspension A is adjusted to obtain a gallium oxyhydroxide precipitate suspension B, and the gallium oxyhydroxide precipitate suspension B is transported to an atomizing nozzle under continuous stirring, atomized into droplets by an atomizing gas medium, and the droplets are spheroidized by plasma to obtain the obtained product; The purity of the metal Ga is ≥5N; The resistivity of the ultrapure water is not less than 18 MΩ.cm at 25°C; The gallium oxyhydroxide precipitate suspension B, the mass ratio of gallium oxyhydroxide precipitate to water is 10 to 15: 90 to 85; The pressure of the atomizing gas medium is 1.6-2.2MPa; the flow rate of the atomizing gas medium is 0.5L / min~2.5L / min; When the plasma is spheroidized, the power of the plasma is 9.75KW~12.8KW.

2. The method for preparing high-purity β-gallium oxide nanospheres according to claim 1, characterized in that: The mass ratio of the metal Ga to ultrapure water is 1:2-10.

3. The method for preparing high-purity β-gallium oxide nanospheres according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180-280° C., and the time of the hydrothermal reaction is 5-8 hours.

4. The method for preparing high-purity β-gallium oxide nanospheres according to claim 1, characterized in that: The atomizing gas medium is selected from argon with a purity of ≥5N.

5. A high-purity β-gallium oxide nanoparticle prepared by the preparation method according to any one of claims 1 to 4.

6. The high-purity β-gallium oxide nanosphere according to claim 5, characterized in that: The purity of the high-purity β-gallium oxide nano-microspheres is ≥5N, and the particle size of the high-purity β-gallium oxide nano-microspheres is 100-500nm.