Preparation method of TiZrVNbAl alloy powder with high fine powder yield
By using the suspension smelting water-cooled crucible atomization powder making process in the preparation of TiZrVNbAl alloy powder, adjusting the diversion pipe and nozzle structure, the problem of insufficient fine powder collection rate in the prior art is solved, and high fine powder collection rate is achieved and improve spherical shape to meet the particle size requirements of additive manufacturing.
Patent Information
- Application Number
- CN202411415718.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-17
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The existing powder preparation technology is difficult to achieve high fine powder yield in TiZrVNbAl alloys, limiting its wide application in additive manufacturing.
The air atomization powder making process of suspended smelting water-cooled crucible is adopted. By coupling the diversion pipe and nozzle structure, the diameter, heating power, nozzle shape and position are adjusted, and the interaction between gas and fluid is improved, ensuring high-temperature fine fluids. Formation and effective atomization.
The fine powder yield of TiZrVNbAl alloy powder is improved, and a high spherical shape and suitable particle size distribution are obtained to meet the performance requirements of additive manufacturing.
Smart Images

Figure CN119140832A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing TiZrVNbAl alloy powder with a high fine powder yield, belonging to the technical field of alloy powder materials. Background Art
[0002] TiZrVNbAl alloy is a representative lightweight high-entropy alloy, which features high specific strength, excellent strength and toughness, good high-temperature stability, and outstanding corrosion resistance. These properties enable it to exhibit broad application prospects in fields such as aerospace, automotive, and energy. To fabricate high-performance complex components of TiZrVNbAl alloy, additive manufacturing technology is an effective technical approach. During the additive manufacturing process, metal powder, as the key raw material, directly affects the performance and reliability of the final components. Therefore, there are relatively high requirements for metal powder, including high sphericity, high fluidity, and high fine powder yield, etc.
[0003] However, due to the characteristics of TiZrVNbAl alloy such as high melting point, high activity, and poor fluidity, the existing powder preparation technologies face certain challenges. Currently, although traditional electrode induction gas atomization process and emerging levitation melting water-cooled crucible gas atomization process can meet the requirements of high sphericity and high fluidity, there are still obvious deficiencies in the fine powder yield, which limits the wide application of TiZrVNbAl alloy in additive manufacturing. Summary of the Invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing TiZrVNbAl alloy powder with a high fine powder yield. The present invention adopts the levitation melting water-cooled crucible gas atomization powder preparation process, and conducts a coupled design on the structures of the flow guide tube and nozzle in the gas atomization powder preparation process to prepare TiZrVNbAl alloy powder with a high fine powder yield.
[0005] To achieve the above purpose, the technical solution of the present invention is as follows.
[0006] A method for preparing TiZrVNbAl alloy powder with a high fine powder yield, the method steps include:
[0007] (1) Determine the alloy composition: The chemical composition and atomic percentage of the lightweight high-entropy alloy TiZrVNbAl are Ti a Zr b V c Nb d Al e , where 25 ≤ a ≤ 60%, 5 ≤ b ≤ 30%, 5 ≤ c ≤ 20%, 10 ≤ d ≤ 25%, 0 < e ≤ 10%, and a + b + c + d + e = 100%;
[0008] (2) Pre-alloying: weighing the metal blocks of each element according to the alloy composition and proportion and adding them into a suspension smelting water-cooled copper crucible, evacuating the water-cooled copper crucible, and then introducing an inert gas to melt the metal blocks in the water-cooled copper crucible. After melting, condensing the metal blocks to obtain alloy ingots;
[0009] (3) Cold crucible smelting: the alloy ingot is added back into the water-cooled copper crucible, evacuated, and then an inert gas is introduced to heat and melt the alloy ingot. When the alloy ingot is completely melted, it is kept at 1700-1750°C, and the guide tube connected to the bottom of the water-cooled copper crucible is heated; wherein the diameter of the guide tube is 2-5 mm;
[0010] (4) Atomization powder making: After the temperature of the guide tube reaches 1700-1750°C, the atomizing gas is turned on for atomization powder making. The alloy melt flowing out from the bottom of the guide tube is impacted and broken into small droplets and solidified to form powder. The atomizing nozzle is an annular structure, the nozzle outlet gap size is 0.8-1.2 mm, the nozzle is aligned with the guide tube outlet, and the angle between the guide tube and the nozzle is 50°-60°. The atomizing gas pressure is 4-8 MPa.
[0011] (5) After the atomization powder making is completed, cooling and screening are performed to obtain a TiZrVNbAl alloy powder with a high fine powder yield.
[0012] Preferably, in step (1), 35%≤a≤55%, 10≤b≤25%, 8≤c≤15%, 10≤d≤20%, and 1≤e≤7%.
[0013] Preferably, in step (2), the purity of the metal block is greater than 99%.
[0014] Preferably, in step (2), the vacuum is evacuated to 5×10 -3 Below Pa.
[0015] Preferably, in step (2), the diameter of the flow guide tube is 3 to 4 mm.
[0016] Preferably, in step (3), the vacuum is evacuated to 2×10 -2 Below Pa.
[0017] Preferably, in step (4), the nozzle outlet gap size is 0.9 to 1.0 mm.
[0018] Preferably, in step (4), the atomizing gas pressure is 5 to 6 MPa.
[0019] Preferably, the inert gas is argon.
[0020] A TiZrVNbAl alloy powder with high fine powder yield is prepared by the above method.
[0021] Beneficial Effects
[0022] The present invention provides a method for preparing TiZrVNbAl alloy powder with a high fine powder yield, by designing the diameter of the guide tube in the gas atomization powder making process. A high-temperature fine fluid is obtained by appropriately reducing the diameter of the guide tube and increasing the heating power at the bottom of the crucible; at the same time, the geometric shape and position of the nozzle in the gas atomization powder making process are designed, and an annular nozzle is used to enhance the coupling effect with the fluid flowing out of the guide tube. The pores of the annular nozzle are adjusted to match the diameter of the guide tube, reduce the resistance to fluid flow, and further enhance the interaction between the gas and the fluid. The relative position and angle between the nozzle and the guide tube are adjusted to ensure better contact between the atomizing gas and the fluid, so that the gas can more effectively atomize the fluid to form finer droplets, thereby increasing the fine powder rate.
[0023] The present invention provides a method for preparing TiZrVNbAl alloy powder with high fine powder yield, and the flow rate matching design is performed on the flow guide tube and the nozzle in the gas atomization powder making process, and the pressure of the atomizing gas is adjusted to ensure that the gas speed is high enough, so that the liquid can be effectively atomized while preventing the droplets from being too large. The outflow speed of the fluid in the flow guide tube is accurately controlled by a flow control valve to match the flow rate of the atomizing gas, which provides a more stable fluid flow path, reduces the turbulence and instability of the fluid flow, helps to control the size and shape of the particles, and improves the yield of fine powder.
[0024] The invention provides a TiZrVNbAl alloy powder with a high fine powder yield. The obtained high-temperature fine fluid has a high temperature and a low viscosity, so the formed powder particles are not prone to agglomeration, which helps to obtain a powder with high sphericity and increases the sphericity of the powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 1 of the present invention 40 Zr 20 V 15 Nb 20 Al 5 SEM image of alloy powder;
[0026] Figure 2 The method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 1 of the present invention is as follows: 40 Zr 20 V 15 Nb 20 Al 5 Laser particle size distribution diagram of alloy powder;
[0027] Figure 3 A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 2 of the present invention 50 Zr 20 V 15 Nb 10 Al 5 SEM image of alloy powder;
[0028] Figure 4 The method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 2 of the present invention is as follows: 50 Zr 20 V 15 Nb 10 Al 5 Laser particle size distribution of alloy powder.
[0029] Figure 5 A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 3 of the present invention 50 Zr 15 V 10 Nb 20 Al 5 SEM image of alloy powder;
[0030] Figure 6 The method for preparing a TiZrVNbAl alloy powder with a high fine powder yield provided in Example 3 of the present invention is as follows: 50 Zr 15 V 10 Nb 20 Al 5 Laser particle size distribution of alloy powder. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with specific embodiments.
[0032] A method for preparing TiZrVNbAl alloy powder with high fine powder yield, the method steps comprising:
[0033] (1) Determine the alloy composition: The alloy components are selected from Ti, Zr, V, Nb, and Al. The ratio of each element is set according to the alloy atomic ratio or mass ratio. The chemical composition and atomic percentage of the lightweight high entropy alloy are Ti a Zr b V c Nb d Al e; wherein, 25 ≤ a ≤ 60%, 5 ≤ b ≤ 30%, 5 ≤ c ≤ 20%, 10 ≤ d ≤ 25%, 0 < e ≤ 10%, and a + b + c + d + e = 100%. More preferably, 35% ≤ a ≤ 55%, 10 ≤ b ≤ 25%, 8 ≤ c ≤ 15%, 10 ≤ d ≤ 20%, 1 ≤ e ≤ 7%.
[0034] (2) Pre-alloying: Determine the required metal blocks according to the alloy composition and ratio, and the purity of the metal blocks is greater than 99%. Add the metal blocks into a suspended melting water-cooled copper crucible, evacuate to below 5×10 -3 Pa, and introduce argon gas into the crucible. Melt the metal blocks in the water-cooled copper crucible, and perform condensation after melting to obtain alloy ingots.
[0035] (3) Cold crucible melting: Put the alloy ingots back into the water-cooled copper crucible. Evacuate the inside of the water-cooled copper crucible to below 2×10 -2 Pa, and then fill it with the inert gas argon. Heat up the alloy ingots, and preheat the diversion tube connected to the bottom of the water-cooled copper crucible. Keep the temperature at 1700 - 1750°C for insulation after the alloy ingots are completely melted, and continuously heat the diversion tube.
[0036] (4) Atomization powder making: When the temperature in the diversion tube reaches 1700 - 1750°C, turn on the atomization gas, and set the pressure of the atomization gas to 4 - 8 MPa. The atomization gas uses argon with a purity greater than or equal to 99.99%, and the content of other impurities in the gas is less than 10 ppm. The inner diameter of the diversion tube is set at 2 - 5 mm, the size of the outlet gap of the annular nozzle is set at 0.8 - 1.2 mm, the nozzle is aligned with the diversion tube, and the angle between the diversion tube and the nozzle is set at 50° - 60°. The alloy liquid in the crucible flows into the diversion tube. The high-pressure atomization gas released by the annular nozzle impacts the alloy melt flowing out from the end of the diversion tube, causing the melt to break into small droplets. Design the flow rate matching for both, and by adjusting the pressure of the atomization gas, ensure that the speed of the atomization gas is high enough to effectively atomize the fluid. Precisely control the outflow speed of the fluid in the diversion tube through a flow control valve to match it with the flow rate of the atomization gas and enhance the interaction between the two.
[0037] (5) Cooling and screening: The fine droplets solidify into spherical particles and sub-spherical particles during flight, and then pass through screening to prepare metal powders of various particle sizes.
[0038] Example 1
[0039] Ti 40 Zr 20 V 15 Nb 20 Al 5 Preparation of alloy spherical powder is carried out according to the following steps:
[0040] Alloy Ti 40 Zr 20 V 15 Nb 20 Al 5 The ratio of the elements is in accordance with the following atomic ratio Ti: Zr: V: Nb: Al = 4: 2: 1.5: 2: 0.5, and the purity of the metal block is ≥ 99%. After accurate weighing, the metal block is added to a water-cooled copper crucible, and the water-cooled copper crucible is evacuated to 5×10 -3 Pa, argon gas was introduced into the water-cooled copper crucible.
[0041] Turn on the smelting power supply, melt the metal block in the water-cooled copper crucible, condense it after melting, and obtain an alloy ingot. Put the alloy ingot back into the water-cooled copper crucible. Evacuate the water-cooled copper crucible to 2×10 -2 Pa, and then fill with inert gas argon. The alloy ingot is heated and the guide tube connected to the bottom of the water-cooled copper crucible is preheated. When the alloy ingot is completely melted, it is kept at 1750℃ and the guide tube is continuously heated.
[0042] The diameter of the flow tube is set to 3mm, the outlet gap of the annular nozzle is set to 1.2mm, the nozzle is aligned with the flow tube, and the angle between the flow tube and the nozzle is set to 50°. When the temperature in the flow tube reaches 1750℃, turn on the atomizing gas argon and set the pressure of the atomizing gas to 6MPa. The alloy liquid in the crucible flows into the flow tube. During the atomization process, the high-pressure atomizing gas released through the annular nozzle impacts the alloy melt flowing out of the end of the flow tube, causing the melt to break into small droplets. The tiny droplets solidify into spherical particles and sub-spherical particles in flight. After the powder particles are cooled, the powder particles are sieved to obtain Ti of the desired particle size. 40 Zr 10 V 10 Nb 10 Al 5 Alloy spherical powder.
[0043] The Ti prepared by this method 40 Zr 20 V 15 Nb 20 Al 5 Powder morphology Figure 1 As shown, it can be seen that the powder morphology is spherical. After screening, the powder particle size distribution is as follows Figure 2 As shown, the D10 of the powder is 9.191 μm, the D50 is 13.940 μm, and the D90 is 20.980 μm. The fine powder rate is high, which meets the powder particle size requirements used in the additive manufacturing process.
[0044] Example 2
[0045] Ti 50 Zr20 V 15 Nb 10 Al 5 The alloy spherical powder is prepared according to the following steps:
[0046] Alloy Ti 50 Zr 20 V 15 Nb 10 Al 5 The ratio of elements in the suspension melting chamber is in accordance with the following atomic ratio Ti: Zr: V: Nb: Al = 5: 2: 1.5: 1: 0.5, and the purity of the metal block is ≥ 99%. After accurate weighing, the metal block is added to the suspension melting water-cooled copper crucible in the suspension melting chamber, and the suspension melting chamber is evacuated to 5×10 -3 Below Pa, argon gas is introduced into the suspension smelting chamber.
[0047] Turn on the smelting power supply, melt the metal block in the water-cooled copper crucible, condense it after melting, and obtain an alloy ingot. Put the alloy ingot back into the water-cooled copper crucible. Evacuate the water-cooled copper crucible to 2×10 -2 Pa, and then fill with inert gas argon. The alloy ingot is heated and the guide tube connected to the bottom of the water-cooled copper crucible is preheated. When the alloy ingot is completely melted, it is kept at 1700℃ and the guide tube is continuously heated.
[0048] The diameter of the flow tube is set to 4mm, the outlet gap of the annular nozzle is set to 1.0mm, the nozzle is aligned with the flow tube, and the angle between the flow tube and the nozzle is set to 55°. When the temperature in the flow tube reaches 1700℃, turn on the atomizing gas argon and set the pressure of the atomizing gas to 4MPa. The alloy liquid in the crucible flows into the flow tube. During the atomization process, the high-pressure atomizing gas released through the annular nozzle impacts the alloy melt flowing out of the end of the flow tube, causing the melt to break into small droplets. The tiny droplets solidify into spherical particles and sub-spherical particles in flight. After the powder particles are cooled, the powder particles are sieved to obtain Ti of the desired particle size. 50 Zr 20 V 15 Nb 10 Al 5 Alloy spherical powder.
[0049] The Ti prepared by this method 50 Zr 20 V 15 Nb 10 Al 5 Powder morphology Figure 3 As shown, it can be seen that the powder morphology is spherical. After screening, the powder particle size distribution is as follows Figure 4As shown in the figure, the D10, D50 and D90 of the powder are 14.921μm, 24.840μm and 41.941μm, respectively. The fine powder rate is high, which meets the powder particle size requirements for additive manufacturing processes.
[0050] Example 3
[0051] Ti 50 Zr 15 V 10 Nb 20 Al 5 The alloy spherical powder is prepared according to the following steps:
[0052] Alloy Ti 50 Zr 15 V 10 Nb 20 Al 5 The ratio of elements in the suspension melting chamber is in accordance with the following atomic ratio Ti: Zr: V: Nb: Al = 5: 1.5: 1: 2: 0.5, and the purity of the metal block is ≥ 99%. After accurate weighing, the metal block is added to the suspension melting water-cooled copper crucible in the suspension melting chamber, and the suspension melting chamber is evacuated to 5×10 -3 Below Pa, argon gas is introduced into the suspension smelting chamber.
[0053] Turn on the smelting power supply, melt the metal block in the water-cooled copper crucible, condense it after melting, and obtain an alloy ingot. Put the alloy ingot back into the water-cooled copper crucible. Evacuate the water-cooled copper crucible to 2×10 -2 Pa, and then fill with inert gas argon. The alloy ingot is heated and the guide tube connected to the bottom of the water-cooled copper crucible is preheated. When the alloy ingot is completely melted, it is kept at 1700℃ and the guide tube is continuously heated.
[0054] The diameter of the flow tube is set to 5mm, the outlet gap of the annular nozzle is set to 0.8mm, the nozzle is aligned with the flow tube, and the angle between the flow tube and the nozzle is set to 55°. When the temperature in the flow tube reaches 1700℃, turn on the atomizing gas argon and set the pressure of the atomizing gas to 4MPa. The alloy liquid in the crucible flows into the flow tube. During the atomization process, the high-pressure atomizing gas released through the annular nozzle impacts the alloy melt flowing out of the end of the flow tube, causing the melt to break into small droplets. The tiny droplets solidify into spherical particles and sub-spherical particles in flight. After the powder particles are cooled, the powder particles are sieved to obtain Ti of the desired particle size. 50 Zr 15 V 10 Nb 20 Al 5 Alloy spherical powder.
[0055] The Ti prepared by this method 50 Zr15 V 10 Nb 20 Al 5 Powder morphology Figure 5 As shown, it can be seen that the powder morphology is spherical. After screening, the powder particle size distribution is as follows Figure 6 As shown in the figure, the D10 of the powder is 17.623μm, the D50 is 30.377μm, and the D90 is 53.077μm. It has an excellent fine powder rate and meets the powder particle size requirements for additive manufacturing processes.
[0056] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A method for preparing TiZrVNbAl alloy powder with high fine powder yield, Features: The method steps include: (1) Determine the alloy composition: The chemical composition and atomic percentage of the lightweight high-entropy alloy TiZrVNbAl are Ti a Zr b V c Nb d Al e , where 25 ≤ a ≤ 60%, 5 ≤ b ≤ 30%, 5 ≤ c ≤ 20%, 10 ≤ d ≤ 25%, 0 < e ≤ 10%, and a + b + c + d + e = 100%; (2) Pre-alloying: weighing the metal blocks of each element according to the alloy composition and proportion and adding them into a suspension smelting water-cooled copper crucible, evacuating the water-cooled copper crucible, and then introducing an inert gas to melt the metal blocks in the water-cooled copper crucible. After melting, condensing the metal blocks to obtain alloy ingots; (3) Cold crucible smelting: the alloy ingot is added back into the water-cooled copper crucible, evacuated, and then an inert gas is introduced to heat and melt the alloy ingot. When the alloy ingot is completely melted, it is kept at 1700-1750°C, and the guide tube connected to the bottom of the water-cooled copper crucible is heated; wherein the diameter of the guide tube is 2-5 mm; (4) Atomization powder making: After the temperature of the guide tube reaches 1700-1750°C, the atomizing gas is turned on for atomization powder making. The alloy melt flowing out from the bottom of the guide tube is impacted and broken into small droplets and solidified to form powder. The atomizing nozzle is an annular structure, the nozzle outlet gap size is 0.8-1.2 mm, the nozzle is aligned with the guide tube outlet, and the angle between the guide tube and the nozzle is 50°-60°. The atomizing gas pressure is 4-8 MPa. (5) After the atomization powder making is completed, cooling and screening are performed to obtain a TiZrVNbAl alloy powder with a high fine powder yield.
2. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: In step (1), 35%≤a≤55%, 10≤b≤25%, 8≤c≤15%, 10≤d≤20%, and 1≤e≤7%.
3. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: In step (2), the purity of the metal block is greater than 99%.
4. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: In step (2), the vacuum is evacuated to 5×10 -3 Below Pa.
5. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, 3 or 4, Features: In step (2), the diameter of the flow guide tube is 3 to 4 mm.
6. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: In step (3), the vacuum is evacuated to 2×10 -2 Below Pa.
7. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: In step (4), the nozzle outlet gap size is 0.9 to 1.0 mm.
8. A method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1 or 7, Features: In step (4), the atomizing gas pressure is 5 to 6 MPa.
9. The method for preparing a TiZrVNbAl alloy powder with a high fine powder yield as claimed in claim 1, Features: The inert gas is argon.
10. A TiZrVNbAl alloy powder with high fine powder yield, Features: It is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Gas atomization preparation method of fine spherical titanium or titanium alloy powder
CN103846447A
Technique for preparing special Ti6Al4V alloy powder used for material increase manufacturing
CN104148658A
Free falling type nozzle copper-chromium alloy atomization milling process
CN110153438A
Preparation method of high-purity refractory high-entropy alloy spherical powder
CN115815609A
Rare earth aluminum alloy powder applicable for additive manufacturing and preparation method thereof
US20230175102A1
Cited By
Preparation method of aluminum-based alloy powder using CO2 as shielding gas and aluminum-based alloy metal powder
CN119973098A