Preparation method, product and application of silicon dioxide coated ternary material
By using silica to coat ternary materials in lithium-ion batteries, the problem of ternary materials being easily corroded to hydrofluoride is solved. The electrolyte is isolated through the SiO2 layer and HF is consumed, which improves the cycle stability of the battery and electrochemical properties.
Patent Information
- Application Number
- CN202211588846.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The ternary materials in existing lithium-ion batteries are susceptible to damage to hydrofluoride (HF), resulting in unstable material structure and degradation of electrochemical properties.
The preparation method of ternary material coated with silica (SiO2) is adopted to form a SiO2 layer on the surface of the positive electrode material, isolate the electrolyte and react with HF to prevent the dissolution of metal elements and the generation of impurity gases.
It effectively prevents HF from eroding the material surface, improves the material's cycle stability and electrochemical performance, and extends the battery's cycle life.
Smart Images

Figure 221212143402
Abstract
Description
Technical Field
[0001] The present invention relates to a preparation method of a lithium-ion battery cathode material, in particular to a preparation method, product and application of a ternary material coated with silicon dioxide. Background Art
[0002] As a high specific energy chemical power source, lithium-ion secondary batteries have been widely used in fields such as mobile communication, laptop computers, cameras, camcorders, portable instruments and meters, and have rapidly developed into one of the most important secondary batteries at present. Lithium-ion batteries, as the latest generation of green high-energy storage batteries, have developed rapidly in the early 1990s. Lithium-ion batteries are favored because of their advantages such as high voltage, high energy density, long cycle life, and low environmental pollution.
[0003] Since the ternary material LiNi 1-x-y Co x Mn y O2 (abbreviated as NCM, where 0 < x < 1, 0 < y < 1) has characteristics superior to those of lithium iron phosphate and lithium cobaltate, and different performance ternary electrode materials can be prepared by adjusting the ratios of nickel, cobalt, and manganese. NCM improves the structural stability of the material, enhances the charge-discharge cycle stability and high-temperature stability of the material, and maximally exerts its excellent electrochemical performance.
[0004] Therefore, a novel method for coating a ternary cathode material with SiO2 is needed to further improve the electrochemical performance of the material. Summary of the Invention
[0005] The object of the present invention is to provide a preparation method of a ternary material coated with silicon dioxide.
[0006] Another object of the present invention is to provide a product of a ternary material coated with silicon dioxide prepared by the above method.
[0007] Another object of the present invention is to provide an application of the above product.
[0008] The object of the present invention is achieved through the following scheme: A preparation method of a ternary material coated with silicon dioxide, characterized in that the specific steps of the method are as follows:
[0009] (1) Dissolve nickel isopropoxide and tetrabutyl orthosilicate at 100 mmol: 1-3 mmol in 70 mL of absolute ethanol, perform ultrasonic dispersion for 20-30 min, and then stir for 1-2 h.
[0010] (2) Slowly add 10 mL of deionized water dropwise to the above suspension to form a sol.
[0011] (3) Add lithium salt, cobalt salt and manganese salt to the above sol (the molar ratio of lithium salt, nickel isopropoxide, cobalt salt and manganese salt is 1:1-xy: x:y), stir continuously for 1-2 h, add into a 100 mL reactor, react at 160-180 °C for 10-15 h to obtain a SiO2-coated ternary precursor, wash with deionized water 3-5 times, and dry in a vacuum oven at 60-80 °C.
[0012] (4) Calcine the SiO2-coated ternary precursor at 600-800 °C for 3-5 h to obtain the SiO2-coated ternary material.
[0013] The present invention provides a method for preparing a ternary material coated with silicon dioxide. In order to improve the harmful corrosion of HF to battery materials, coating SiO2 on the surface of the positive electrode material is an effective method. On the one hand, coating SiO2 isolates the positive electrode material from the electrolyte to prevent HF from dissolving the metal elements on the surface of the material; on the other hand, SiO2 can react with a small amount of HF to reduce its corrosion on the electrode surface by consuming HF, reduce the generation of impurity gas, and block the subsequent adverse chain reaction. The present invention provides a novel method for coating ternary positive electrode materials with SiO2, thereby improving the electrochemical performance of the material.
[0014] Based on the above scheme, the lithium salt is one or a combination of lithium hydroxide, lithium acetate or lithium formate.
[0015] The cobalt salt is one of cobalt chloride, cobalt acetate or cobalt formate or a combination thereof.
[0016] The manganese salt is one of manganese chloride, manganese acetate or manganese formate or a combination thereof.
[0017] The present invention provides a silicon dioxide-coated ternary material, which is prepared according to any of the above methods.
[0018] The present invention provides an application of a silicon dioxide-coated ternary material in a lithium battery positive electrode material.
[0019] Beneficial effects of the present invention:
[0020] The SiO2 coating isolates the positive electrode material from the electrolyte, preventing HF from dissolving the metal elements on the surface of the material; in addition, SiO2 can react with a small amount of HF, reducing its corrosion on the electrode surface by consuming HF, reducing the generation of impurity gas, and blocking the subsequent adverse chain reaction. The present invention provides a novel method for coating ternary positive electrode materials with SiO2, thereby improving the electrochemical performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the cycle life diagram of the SiO2-coated ternary material in Example 1. DETAILED DESCRIPTION
[0022] The present invention is described in detail through the following specific examples, but the protection scope of the present invention is not limited to these embodiments.
[0023] Embodiment 1
[0024] A silicon dioxide-coated ternary material is prepared according to the following steps:
[0025] (1) Dissolve nickel isopropoxide and tetrabutyl silicate in 70 mL of anhydrous ethanol at a ratio of 100 mmol:1 mmol and disperse them by ultrasonic for 30 min, then stir for 1 h to obtain a suspension;
[0026] (2) Add 10 mL of deionized water dropwise into the above suspension to form a sol;
[0027] (3) Add lithium hydroxide, cobalt chloride salt and manganese chloride salt to the above sol, wherein the molar ratio of lithium hydroxide, nickel isopropoxide, cobalt chloride and manganese chloride is 1 mmol: 0.333 mmol: 0.333 mmol: 0.333 mmol, and add to a 100 mL reactor after continuous stirring for 1 hour, and react at 160°C for 15 hours to obtain a SiO2-coated ternary precursor, which is washed with deionized water three times and dried in a vacuum oven at 80°C;
[0028] (4) The SiO2-coated ternary precursor was calcined at 600°C for 5 h to obtain the SiO2-coated ternary material.
[0029] The SiO2-coated ternary material was obtained, and the cycle life diagram Figure 1 As shown, its first discharge specific capacity is 178.9 mAh / g. After 50 cycles, the discharge specific capacity is 174.8 mAh / g, and the capacity retention rate is 97.7%.
[0030] Embodiment 2
[0031] A silicon dioxide-coated ternary material is prepared in the following steps similar to those in Example 1:
[0032] (1) Dissolve nickel isopropoxide and tetrabutyl silicate in 70 mL of anhydrous ethanol at a ratio of 100 mmol:2 mmol and perform ultrasonic dispersion for 30 min, then stir for 2 h to obtain a suspension;
[0033] (2) Add 10 mL of deionized water dropwise into the above suspension to form a sol;
[0034] (3) Add lithium acetate, cobalt acetate and manganese acetate to the above sol, wherein the molar ratio of lithium acetate, nickel isopropoxide, cobalt acetate and manganese acetate is 1 mmol: 0.5 mmol: 0.3 mmol: 0.2 mmol. After continuous stirring for 1 h, add the mixture into a 100 mL reactor and react at 170 °C for 12 h to obtain a SiO2-coated ternary precursor. Wash the mixture with deionized water for 5 times and dry it in a vacuum oven at 80 °C.
[0035] (4) The SiO2-coated ternary precursor was calcined at 700 °C for 4 h to obtain the SiO2-coated ternary material.
[0036] Embodiment 3
[0037] A silicon dioxide-coated ternary material is prepared in the following steps similar to those in Example 1:
[0038] (1) Dissolve nickel isopropoxide and tetrabutyl silicate in 70 mL of anhydrous ethanol at a ratio of 100 mmol:3 mmol and perform ultrasonic dispersion for 20 min, then stir for 2 h to obtain a suspension;
[0039] (2) Add 10 mL of deionized water dropwise into the above suspension to form a sol;
[0040] (3) Add lithium formate, cobalt formate and manganese formate to the above sol, wherein the molar ratio of lithium formate, nickel isopropoxide, cobalt formate and manganese formate is 1 mmol: 0.8 mmol: 0.1 mmol: 0.1 mmol, stir continuously for 1 hour, add to a 100 mL reactor, react at 180°C for 10 hours to obtain a SiO2-coated ternary precursor, wash with deionized water 5 times, and dry in a vacuum oven at 60°C;
[0041] (4) The SiO2-coated ternary precursor was calcined at 800°C for 3 h to obtain the SiO2-coated ternary material.
Claims
1. A method for preparing a silicon dioxide-coated ternary material, characterized in that: The silicon dioxide coated ternary material comprises the following preparation steps: (1) Dissolve nickel isopropoxide and tetrabutyl silicate in 70 mL of anhydrous ethanol at a ratio of 100 mmol:1-3 mmol and perform ultrasonic dispersion for 20-30 min, then stir for 1-2 h to obtain a suspension; (2) Add 10 mL of deionized water dropwise into the above suspension to form a sol; (3) Add lithium salt, cobalt salt and manganese salt to the above sol, wherein the molar ratio of lithium salt, nickel isopropoxide, cobalt salt and manganese salt is 1:1-xy:x:y), stir continuously for 1-2 h, add to a 100 mL reactor, react at 160-180 °C for 10-15 h to obtain a SiO2-coated ternary precursor, wash with deionized water 3-5 times, and dry in a vacuum oven at 60-80 °C; (4) Calcine the SiO2-coated ternary precursor at 600-800 °C for 3-5 h to obtain the SiO2-coated ternary material.
2. The method for preparing a silicon dioxide-coated ternary material according to claim 1, characterized in that: The lithium salt is one of lithium hydroxide, lithium acetate or lithium formate or a combination thereof, or the lithium salt is replaced by atmospheric lithium hydroxide.
3. The method for preparing a silicon dioxide-coated ternary material according to claim 1, characterized in that The cobalt salt is one of cobalt chloride, cobalt acetate or cobalt formate or a combination thereof.
4. The method for preparing a silicon dioxide-coated ternary material according to claim 1, characterized in that The manganese salt is one of manganese chloride, manganese acetate or manganese formate or a combination thereof.