A polymer-encapsulated TiO2 composite and its emulsion

By forming a multi-layer cladding layer on the surface of TiO2 and using titanate coupling agent, the dispersion and hiding power of TiO2 are improved, the problems of tight supply and high cost of titanium dioxide are solved, and the amount of titanium dioxide and the production are reduced are achieved. cost effect.

CN115975128BActive Publication Date: 2024-10-15GUANGDONG BADFU NEW MATERIALS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211546937.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-10-15
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

The tight supply of titanium dioxide and high cost in China have caused paint manufacturers to face huge cost pressure, and it is necessary to improve the efficiency of titanium dioxide use or find stronger alternatives to reduce costs.

Method used

Using multi-layer encapsulation technology, the dispersion and covering of TiO2 are improved by forming alkali-swelling polymer and non-alkali-swelling polymer coatings with different refractive indices on the surface of TiO2, combined with dispersant solution and titanate coupling agent. , thereby reducing the amount of titanium dioxide used.

Benefits of technology

It can effectively reduce the amount of titanium dioxide while ensuring the hiding force is unchanged, reduce the production cost of latex paint, and improve the hiding force of the emulsion and the dispersion of TiO2.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a polymer-encapsulated TiO2 composite, and a preparation method thereof comprises the following steps: S1. adding an oxidant solution and a reductant solution to an initial reaction solution containing TiO2; S2. adding a monomer emulsion Me1 to polymerize the monomers contained in the monomer emulsion Me1 to form an alkali-swelling polymer coating layer on the surface of TiO2; S3. adding a monomer emulsion Me2 to polymerize the monomers contained in the monomer emulsion Me2 to form a non-alkali-swelling polymer coating layer covering the alkali-swelling polymer coating layer on the surface of TiO2; S4. adding a neutralizer to adjust Ph to 7.5-8.5, so that the alkali-swelling polymer coating layer and the non-alkali-swelling polymer coating layer swell to different degrees, until the refractive index of the alkali-swelling polymer coating layer is different from the refractive index of the non-alkali-swelling polymer coating layer, so that the emulsion formed by the polymer-encapsulated TiO2 composite has high hiding power.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resin and chemical synthesis, and in particular relates to a polymer-encapsulated TiO2 composite and an emulsion thereof. Background Art

[0002] Water-based interior wall latex paint is a type of water-based paint. It is a water-dispersed system formed by dispersing pigments, fillers and additives in synthetic polymer emulsions. Water-based interior wall latex paint is popular because it uses water as a dispersion medium and has the characteristics of health, environmental protection, convenient construction, good water resistance, and excellent scrub resistance. In recent years, with the development of the national economy and the improvement of people's living standards, the consumption of coatings in my country has been growing steadily.

[0003] Hiding power is one of the important properties of latex paint, reflecting the ability of white and light-colored interior wall latex paint to eliminate the color of the base material. Titanium dioxide is the main factor affecting the hiding power of latex paint. However, due to the shortage of domestic raw titanium ore resources, the supply of titanium dioxide is tight and the price has risen, which has also brought huge cost pressure to paint manufacturers. Therefore, improving the use efficiency of titanium dioxide, reducing the use of titanium dioxide without changing the hiding power, or seeking titanium dioxide with stronger hiding power to reduce costs has become a new idea for the sustainable development of the paint industry. Summary of the invention

[0004] The object of the present invention is to provide a polymer-encapsulated TiO2 complex and an emulsion thereof, so that the emulsion formed by the polymer-encapsulated TiO2 complex has high hiding power.

[0005] According to one aspect of the present invention, there is provided a polymer-encapsulated TiO2 composite, the preparation method of which comprises the following steps:

[0006] S1. Adding an oxidant solution and a reducing agent solution to the initial reaction solution containing TiO2 to obtain a first reaction solution;

[0007] S2. Adding monomer emulsion Me1 to the first reaction liquid to obtain a first mixed liquid, polymerizing the monomers contained in the monomer emulsion Me1 to form an alkali-swellable polymer coating layer on the surface of TiO2, wherein the monomers contained in the monomer emulsion Me1 are alkyl methacrylate and carboxyl-containing unsaturated acid.

[0008] S3. Add monomer emulsion Me2 to the first mixed solution prepared in S2 to prepare a second mixed solution, and polymerize the monomers contained in the monomer emulsion Me2 to form a non-alkali-swellable polymer coating layer coated with an alkali-swellable polymer coating layer on the surface of TiO2, wherein the monomers contained in the monomer emulsion Me2 are alkyl acrylate and styrene.

[0009] S4. Add a neutralizing agent to adjust the Ph of the second mixed solution obtained in S3 to 7.5-8.5, so that the alkali-swelling polymer coating layer and the non-alkali-swelling polymer coating layer swell to different degrees, until the refractive index of the alkali-swelling polymer coating layer is different from the refractive index of the non-alkali-swelling polymer coating layer. In the present invention, by adopting a multi-layer encapsulation technology, TiO2 is uniformly encapsulated in the polymer coating layer, and by adjusting the Ph value, the first layer of alkali-swelling polymer coating layer is stretched and expanded, and a different refractive index is formed between the second layer of non-alkali-swelling polymer coating layer, thereby improving the hiding power of the emulsion.

[0010] Preferably, the preparation method of the above-mentioned initial reaction solution comprises the following steps: according to the mass fraction, 1000 parts of TiO2, 50-90 parts of dispersant solution and 200-300 parts of pure water are mixed, and the slurry thus formed is ground. Since the TiO2 surface contains a large amount of hydroxyl groups, it is easy to reunite, and the covering ability of TiO2 after reunion will be greatly affected. Therefore, TiO2 should be ground more carefully before use, and a certain amount of dispersant is added during the grinding process. The purpose is to separate the TiO2 particles on the one hand, so that the covering ability of TiO2 can be brought into play more. On the other hand, before adding the redox agent and the monomer emulsion, the dispersant is added during the grinding of TiO2. This feeding order makes the dispersant adhere to TiO2 before the polymerization of the alkali swellable polymer and the non-alkali swellable polymer, preventing TiO2 from reunion, thereby improving the dispersion stability of the TiO2 particles.

[0011] Preferably, the slurry formed above is ground in a grinding tank at a speed of 2000 rpm for 20 min, and the solid content of the formed slurry is 76.5%.

[0012] Preferably, calculated by weight, the raw materials for preparing the dispersant solution include 35-75 parts of a monomer solution and 1.5-6 parts of an initiator, wherein the monomer solution includes an acrylamide compound, an acrylate compound, a chain transfer agent and an organic solvent.

[0013] Preferably, the initiator comprises 2,2-azobis(2,4-dimethylvaleronitrile).

[0014] Preferably, the acrylamide compound includes at least one of 2-acrylamido-2-methyl-1-propane sulfonic acid and methacryloyloxyethyl trimethylammonium chloride;

[0015] Preferably, the acrylate compound includes at least one of acrylate monomer and methyl methacrylate;

[0016] Preferably, the acrylate monomer is selected from at least one of n-butyl acrylate and isooctyl acrylate;

[0017] Preferably, the organic solvent is at least one of ethanol, methanol and propanol;

[0018] Preferably, the chain transfer agent is at least one of n-dodecyl mercaptan and n-dodecyl mercaptan benzoate.

[0019] Preferably, calculated by weight, the raw materials for preparing the above-mentioned monomer solution include 5-17 parts of deionized water, 20-60 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid, 4-12 parts of methacryloyloxyethyltrimethylammonium chloride, 10-30 parts of acrylate monomer, 20-40 parts of methyl methacrylate, 20-60 parts of organic solvent, and 1-4 parts of chain transfer agent.

[0020] Preferably, the method for preparing the above dispersant solution comprises the following steps:

[0021] Step a, mixing an acrylamide compound, an acrylate compound, and a chain transfer agent to prepare a monomer solution;

[0022] Step b, adding an initiator to the monomer solution to cause a polymerization reaction in the monomer solution, and using the polymer obtained after the polymerization reaction as a dispersant polymer;

[0023] Step c, extracting a dispersant polymer from the product obtained in step b, and dissolving the dispersant polymer in water, thereby forming a dispersant solution.

[0024] Preferably, in the process of preparing the dispersant solution, the specific operation of step b includes: firstly mixing 35-75 parts of the monomer solution obtained in step a with 0.5-3 parts of initiator, 25-45 parts of organic solvent and 5-15 parts of deionized water at 70°C according to the mass fraction, then heating to 77°C, adding 1-3 parts of initiator and 1-3 parts of organic solvent for the second time, and keeping the temperature for 60 minutes to obtain a polymer as the dispersant polymer. In the present invention, by adding the initiator step by step and slowly heating the temperature step by step, the initiator can be slowly released, and the polymerization reaction can be initiated in stages, which is conducive to improving the stability of the obtained dispersant polymer, thereby improving the dispersant's effect on TiO 2的 Covering power.

[0025] Preferably, in the process of preparing the dispersant solution, the specific operation of step c includes first removing the organic solvent from the dispersant polymer obtained in step b and drying it, then dissolving it in water, and then adding ammonia water to adjust the Ph to 4-6 to obtain the dispersant solution. The dispersant solution is prepared within the above Ph range, which can improve the dispersibility of TiO2. On the one hand, it can reduce the dissociation degree of the dispersant, so that the amount of adsorption on the surface of the TiO2 particles is relatively large, which can give full play to its dispersing effect. On the other hand, it can avoid affecting the synthetic stability of the polymer coating layer encapsulating TiO2.

[0026] Preferably, in step c, the dispersant polymer prepared in step b is subjected to a rotary evaporator to remove the organic solvent.

[0027] Preferably, the oxidant solution in S1 is at least one of hydrogen peroxide and tert-butyl hydroperoxide; the reducing agent solution is at least one of ascorbic acid, isoascorbic acid and sodium bisulfite.

[0028] Preferably, the oxidant solution and the reducing agent solution are added dropwise in S1, wherein the adding time is 100 minutes.

[0029] Preferably, the temperature of S1 to S3 is maintained at 50°C.

[0030] Preferably, the alkyl methacrylate in S2 is at least one of methyl methacrylate, butyl methacrylate, and hydroxyethyl methacrylate; and the carboxyl-containing unsaturated acid in S2 is at least one of methacrylic acid, acrylic acid, and itaconic acid.

[0031] As a further improvement of the above technical solution, calculated according to the mass ratio, methacrylic acid: itaconic acid = 2:1.

[0032] As a further improvement of the above technical solution, calculated by weight, the raw materials for preparing the monomer emulsion Me1 include 100-180 parts of alkyl methacrylate, 10-20 parts of carboxyl-containing unsaturated acid, 5-15 parts of emulsifier, and 50-70 parts of pure water.

[0033] Preferably, the emulsifier is at least one of alkyl polyoxyethylene ether, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate.

[0034] Preferably, the S3 alkyl acrylate is at least one of n-butyl acrylate and isooctyl acrylate.

[0035] Preferably, the S3 alkyl acrylate is n-butyl acrylate. n-Butyl acrylate is more hydrophilic, has a linear structure and a lower Tg, which is conducive to the entry of the neutralizer, and the outermost coating layer may undergo a certain deformation during swelling.

[0036] As a further improvement of the above technical solution, calculated by weight, the raw materials for preparing the monomer emulsion Me2 include 180-250 parts of alkyl acrylate, 120-180 parts of styrene, 25-55 parts of emulsifier, and 90-130 parts of pure water.

[0037] Preferably, the monomer emulsion Me1 is added dropwise in S2, wherein the adding time is 10-30 minutes.

[0038] Preferably, the monomer emulsion Me2 is added dropwise in S3, wherein the adding time is 70-90 minutes.

[0039] Preferably, in step S3, after the monomer emulsion Me2 is added dropwise, the temperature is kept for 60 minutes, and then the temperature is lowered to room temperature before adding the neutralizing agent.

[0040] Preferably, in step S4, 120 parts of a neutralizer are added by weight, wherein the neutralizer includes at least one of sodium hydroxide and potassium hydroxide. Under the above-mentioned neutralizer dosage conditions, the neutralizer can neutralize the carboxyl groups in the alkali-swellable polymer coating layer formed by polymerization of the monomer emulsion Me1, avoiding the situation of insufficient neutralizer.

[0041] In another aspect, an emulsion is provided, comprising the above-mentioned polymer-encapsulated TiO2 composite, wherein the mass of TiO2 in the polymer-encapsulated TiO2 composite accounts for 32.5±0.5% of the total mass of the emulsion, calculated as a percentage by mass.

[0042] Preferably, calculated by mass percentage, the mass of TiO2 in the polymer-encapsulated TiO2 composite accounts for 32.25±0.20% of the total mass of the emulsion.

[0043] Preferably, the emulsion further comprises a titanate coupling agent, and calculated by mass percentage, the mass of the titanate coupling agent accounts for 0.18-0.35% of the total mass of the emulsion.

[0044] Preferably, the titanate coupling agent includes at least one of isopropyl tri(dioctyl pyrophosphate) titanate, isopropyl dioleyloxy(dioctyl pyrophosphate) titanate, and bis(dioctyl pyrophosphate) ethylene titanate.

[0045] Preferably, the emulsion includes 120 parts of a neutralizer and 4-10 parts of a titanate coupling agent, calculated by weight ratio. In the present invention, by adding a titanate coupling agent, the titanate coupling agent is cross-linked to the surface of TiO2 to exert a synergistic effect, the purpose of which is to improve the modification effect of the polymer encapsulation on the surface of TiO2, so that the modified TiO2 has good dispersibility and is not easy to agglomerate, thereby improving the hiding power of TiO2.

[0046] In summary, compared with the prior art, the solution provided by the present invention has the following beneficial effects:

[0047] (1) The present invention adopts multi-layer encapsulation technology to uniformly encapsulate TiO2 in the polymer coating layer. By adjusting the Ph value, the first alkali-swellable polymer coating layer is stretched and expanded to form a different refractive index with the second non-alkali-swellable polymer coating layer, thereby improving the hiding power of the emulsion;

[0048] (2) The present invention uses a dispersant solution and a titanate coupling agent to make TiO2 have good dispersibility and be difficult to agglomerate, thereby further improving the hiding power of the emulsion;

[0049] (3) The polymer-encapsulated TiO2 composite provided by the present invention can effectively reduce the amount of titanium dioxide in latex paint while ensuring the hiding power remains unchanged, thereby reducing the production cost of latex paint. DETAILED DESCRIPTION

[0050] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0051] Example 1

[0052] Treatment Group 1

[0053] A polymer-encapsulated TiO2 composite and its emulsion, wherein the preparation method comprises the following steps:

[0054] (1) Preparation of dispersant:

[0055] Step a) Preparation of a monomer solution: 14 parts of deionized water, 40 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid, 8 parts of methacryloyloxyethyl trimethylammonium chloride, 20 parts of n-butyl acrylate, 30 parts of methyl methacrylate, 40 parts of anhydrous ethanol, and 2 parts of n-dodecyl mercaptan are weighed according to mass fractions, added into a monomer tank equipped with a stirrer, stirred for 10-15 minutes to mix evenly for later use, to prepare a monomer solution;

[0056] Step b) Add 12 parts of deionized water, 35 parts of anhydrous ethanol, 55 parts of the monomer solution prepared in step a), and 1.3 parts of 2,2-azobis(2,4-dimethylvaleronitrile) to a four-necked flask equipped with a stirrer, a condenser, and a constant flow pump feeding device, and heat the flask until the temperature reaches 55° C., turn off the heating, and allow the system to naturally exotherm and heat up;

[0057] Step c) After the exotherm of step b) reaches a peak value, heating is turned on to keep the system temperature in the four-necked flask at 70° C., and the remaining monomer solution is added for 1 hour; after the monomer solution is added, the temperature is kept at 70° C. for 60 minutes; then the temperature is raised to 77° C., 1.5 parts of 2,2-azobis(2,4-dimethylvaleronitrile) and 2 parts of anhydrous ethanol are added to the flask, and the temperature is kept for another 60 minutes to polymerize the monomer solution to obtain a dispersant polymer;

[0058] Step d) cooling the four-necked flask to room temperature, removing the organic solvent by a rotary evaporator, collecting the dispersant polymer prepared in step c) and drying it, then dissolving the dispersant polymer in water and adding ammonia water to adjust the Ph to 4-6, to prepare a dispersant solution with a Ph of 4-6 and a mass fraction of 21%;

[0059] (2) Preparation of TiO2 slurry:

[0060] Add 72 parts of the above prepared dispersant solution, 240 parts of pure water, and 1000 parts of TiO2 into a steel grinding jar. Slowly add TiO2 while grinding at a speed of 2000 rpm. After adding TiO2, grind the slurry for 20 minutes. The solid content of the slurry is 76.5%.

[0061] (3) Synthesis of TiO2 polymer coating:

[0062] Step e) Preparation of monomer emulsion Me1: according to the mass fractions, 60 parts of pure water, 11 parts of sodium dodecylbenzene sulfonate, 62 parts of methyl methacrylate, 85 parts of n-butyl methacrylate, 10 parts of acrylic acid, and 5 parts of itaconic acid were weighed and added into an emulsification tank, mixed evenly and set aside;

[0063] Step f) Preparation of monomer emulsion Me2: According to the mass fractions, 110 parts of pure water, 45 parts of sodium dodecylbenzene sulfonate, 215 parts of n-butyl acrylate, and 156 parts of styrene are weighed and added into an emulsification tank, and mixed evenly for later use;

[0064] Step g) Add 165 parts of pure water and 1085 parts of the prepared TiO2 slurry into a four-necked flask equipped with a condensing device, a stirring device and a feeding device, and heat the system to and maintain it at 50°C;

[0065] Step h) When the temperature of the four-necked flask is maintained at 50° C., the oxidant solution and the reducing agent solution are added dropwise at the same time, and the adding time is 100 min. The monomer emulsion Me1 is added dropwise for 20 min, and the monomer emulsion Me2 is added dropwise for 80 min. Calculated by weight, the oxidant solution includes 11 parts of tert-butyl hydroperoxide and 200 parts of pure water, and the reducing agent solution includes 6 parts of ascorbic acid and 200 parts of pure water.

[0066] Step i) After the monomer emulsion Me2 is added dropwise, the mixture is kept warm for 60 minutes, then cooled to room temperature and 120 parts by weight of a 5% sodium hydroxide neutralizer is added dropwise within 30 minutes to obtain a polymer-encapsulated composite.

[0067] Step j) 6 parts of titanate coupling agent are added, and the material is filtered to obtain an emulsion formed by a polymer-encapsulated TiO2 composite.

[0068] Treatment Group 2

[0069] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and the treatment group 1 of this embodiment is that this treatment group omits step j) of the treatment group 1 of this embodiment to add the titanate coupling agent. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of the treatment group 1 of this embodiment.

[0070] Comparative treatment group 1

[0071] The comparative treatment group prepared the polymer-encapsulated TiO2 composite and its emulsion with reference to the treatment group 1 of the present embodiment. The difference between the comparative treatment group and the treatment group 1 of the present embodiment is that the comparative treatment group omitted the addition of 120 parts of sodium hydroxide neutralizer in step i) of the treatment group 1 of the present embodiment, that is, the Ph of the second mixed solution was not adjusted. In addition to the above differences, the materials and process operations used in the comparative treatment group were strictly consistent with those of the treatment group 1 of the present embodiment.

[0072] Comparative treatment group 2

[0073] The comparative treatment group prepared the polymer-encapsulated TiO2 composite and its emulsion with reference to the treatment group 1 of the present embodiment. The difference between the comparative treatment group and the treatment group 1 of the present embodiment 1 is that the comparative treatment group replaced the addition of 120 parts of sodium hydroxide neutralizer in step i) of the treatment group 1 of the present embodiment with the addition of 80 parts of sodium hydroxide neutralizer. In addition to the above differences, the materials and process operations used in the comparative treatment group are strictly consistent with those of the treatment group 1 of the present embodiment.

[0074] Comparative treatment group 3

[0075] The comparative treatment group prepared the polymer-encapsulated TiO2 composite and its emulsion with reference to the treatment group 1 of the present embodiment. The difference between the comparative treatment group and the treatment group 1 of the present embodiment is that the comparative treatment group replaced the addition of 120 parts of sodium hydroxide neutralizer in step i) of the treatment group 1 of the present embodiment with the addition of 140 parts of sodium hydroxide neutralizer. In addition to the above differences, the materials and process operations used in the comparative treatment group are strictly consistent with those of the treatment group 1 of the present embodiment.

[0076] Comparative treatment group 4

[0077] The comparative treatment group refers to the treatment group 1 of the present embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between the comparative treatment group and the treatment group 1 of the present embodiment is that the comparative treatment group omits the step e) preparation of the monomer emulsion Me2 of the treatment group 1 of the present embodiment, that is, only one alkali-swelling polymer coating layer is formed on the TiO2 surface. In addition to the above differences, the materials and process operations used in the comparative treatment group are strictly consistent with those of the treatment group 1 of the present embodiment.

[0078] Comparative treatment group 5

[0079] The comparative treatment group refers to the treatment group 1 of the present embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between the comparative treatment group and the treatment group 1 of the present embodiment is that the comparative treatment group omits the step f) of the treatment group 1 of the present embodiment to prepare the monomer emulsion Me1, that is, only a non-alkali swelling polymer coating layer is formed on the TiO2 surface. In addition to the above differences, the materials and process operations used in the comparative treatment group are strictly consistent with those of the treatment group 1 of the present embodiment.

[0080] Test Example 1

[0081] 1. Test objects: polymer-encapsulated TiO2 composites and their emulsions obtained from treatment groups 1-2 and comparative treatment groups 1-5 of Example 1.

[0082] 2. Test method: The emulsions formed by the polymer-encapsulated TiO2 complex obtained in treatment groups 1 to 2 of Example 1 and comparative treatment groups 1 to 5 were respectively prepared according to the formula compositions shown in Table 1, and the prepared paints were subjected to performance tests according to the international standard GB / T9756-2018.

[0083] Table 1. Formula components used to prepare latex paint

[0084]

[0085]

[0086] 3. Test results analysis

[0087] The performance test results are shown in Table 2, where the contrast ratio is the ratio of the whiteness of the black base and the white base after the paint film is applied. The higher the value, the stronger the hiding power. As shown in Table 2, the use of titanate coupling agent in the emulsion formed by the polymer encapsulated TiO2 composite, the addition of a neutralizer to adjust the Ph to 7.5-8.5, and the provision of a first alkali-swellable polymer coating layer and a second non-alkali-swellable polymer coating layer on the TiO2 surface can have a certain impact on the hiding power performance of the emulsion.

[0088] Comparing the corresponding performance test results of treatment group 1 and treatment group 2 of Example 1, the paint film formed by the emulsion using titanate coupling agent as a component under the conditions where other components and their proportions are the same has a higher wet film contrast ratio and dry film contrast ratio.

[0089] The corresponding performance test results of treatment group 1 in Example 1 and comparison treatment groups 1 to 3 in Table 2 were compared. Under the conditions of preparing other components and their proportions of latex paint being the same, the paint film formed by the emulsion in which the Ph was adjusted to 7.5-8.5 by adding a neutralizer had a higher wet film contrast ratio and dry film contrast ratio, that is, the emulsion formed by the polymer-encapsulated TiO2 complex had a high hiding power.

[0090] Comparing the treatment group 1 of Example 1 with the comparative treatment groups 4-5, when the other components and their proportions of the latex paint are the same, the wet film contrast ratio and dry film contrast ratio of the paint film formed by the emulsion in which only one monomer emulsion Me1 or Me2 is added as the formula component are significantly lower than the paint film formed by the emulsion in which both monomer emulsion Me1 and monomer emulsion ME2 are added as the formula components. The above results show that the paint film formed by the emulsion in which the first alkali-swelling polymer coating layer and the second non-alkali-swelling polymer coating layer are respectively arranged on the surface of TiO2 has a higher wet film contrast ratio and dry film contrast ratio, because the first alkali-swelling polymer coating layer and the second non-alkali-swelling polymer coating layer swell to different degrees under weak alkaline conditions, so that the refractive index of the alkali-swelling polymer coating layer is different from the refractive index of the non-alkali-swelling polymer coating layer, so that the emulsion formed by the polymer-encapsulated TiO2 complex has a higher hiding power.

[0091] Table 2. Performance test results of Example 1

[0092]

[0093] Example 2

[0094] Treatment Group 1

[0095] This treatment group prepared the polymer-encapsulated TiO2 composite and its emulsion according to the treatment group 1 of Example 1. The materials and process operations used in this treatment group were strictly consistent with those of the treatment group 1 of Example 1.

[0096] Treatment Group 2

[0097] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that this treatment group omits the preparation of the dispersant in step a) of treatment group 1, and directly adds TiO2 to the grinding tank for grinding to obtain TiO2 slurry. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those of treatment group 1 of this embodiment.

[0098] Treatment Group 3

[0099] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that this treatment group omits the step a) of using 40 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid and 8 parts of methacryloyloxyethyl trimethyl ammonium chloride to prepare the monomer solution in treatment group 1. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those of treatment group 1 of this embodiment.

[0100] Treatment Group 4

[0101] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that this treatment group omits the step a) of using 20 parts of n-butyl acrylate and 30 parts of methyl methacrylate to prepare the monomer solution in treatment group 1. Except for the above differences, the materials and process operations used in this embodiment are strictly consistent with those of treatment group 1 of this embodiment.

[0102] Treatment Group 5

[0103] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and the treatment group 1 of this embodiment is that this treatment group replaces the addition of 2,2-azobis(2,4-dimethylvaleronitrile) to the reaction system twice in steps b) and c) of the treatment group 1 of this embodiment with the direct addition of 2.8 parts of 2,2-azobis(2,4-dimethylvaleronitrile) to the reaction system at one time. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of the treatment group 1 of this embodiment.

[0104] Treatment Group 6

[0105] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer encapsulated TiO2 composite and its emulsion. The difference between this treatment group and the treatment group 1 of this embodiment is that this treatment group omits the step d) of adding ammonia water to adjust Ph to 4-6 in the treatment group 1 of this embodiment. Except for the above differences, the materials and process operations used in this treatment group are strictly consistent with those of the treatment group 1 of this embodiment.

[0106] Test Example 2

[0107] 1. Test objects: polymer-encapsulated TiO2 composites and their emulsions obtained from treatment groups 1 to 6 of Example 2.

[0108] 2. Test method: The test method refers to the test method performed in Test Example 1.

[0109] 3. Test result analysis:

[0110] The performance test results are shown in Table 3. As can be seen from Table 3, the performance test results of the emulsion formed by the polymer-encapsulated TiO2 complex of treatment groups 1 to 6 in Example 2 are shown in Table 3. As can be seen from Table 3, relative to treatment groups 2 to 6, the polymer-encapsulated TiO2 complex and its emulsion provided by the present invention have excellent hiding power by adding a dispersant solution, rationally setting the components of the dispersant solution and the preparation operation. And relative to treatment group 2, the emulsion formed by the polymer-encapsulated TiO2 complex provided by treatment group 1 can improve the hiding power of the emulsion by adding a dispersant solution. Relative to treatment groups 3 to 4, the emulsion formed by the polymer-encapsulated TiO2 complex provided by treatment group 1 has better hiding power by adding a dispersant containing acrylamide compounds and acrylate compounds. Relative to treatment group 5, the polymer-encapsulated TiO2 complex and its emulsion provided by treatment group 1 have better dispersibility by adding an initiator in the process of preparing the dispersant, so that the obtained dispersant solution has better dispersibility, thereby making the emulsion have excellent hiding power. Compared with treatment group 6, the polymer-encapsulated TiO2 complex and its emulsion provided by treatment group 1 can fully exert the dispersing effect of the dispersant solution on TiO2 by adjusting Ph by adding ammonia water during the preparation of the dispersant, further improving the covering power of the emulsion.

[0111] Table 3. Performance test results of Example 2

[0112]

[0113] Example 3

[0114] Treatment Group 1

[0115] This treatment group prepared the polymer-encapsulated TiO2 composite and its emulsion according to the treatment group 1 of Example 1. The materials and process operations used in this treatment group were strictly consistent with those of the treatment group 1 of Example 1.

[0116] Treatment Group 2

[0117] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that in step e) of treatment group 1, 62 parts of methyl methacrylate and 85 parts of n-butyl methacrylate are used to prepare the monomer emulsion Me1, which is replaced by 90 parts of methyl methacrylate and 45 parts of hydroxyethyl methacrylate. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of treatment group 1 of this embodiment.

[0118] Treatment Group 3

[0119] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between this treatment group and the treatment group 1 is that in the step e) of the treatment group 1, 62 parts of methyl methacrylate and 85 parts of n-butyl methacrylate are used to prepare the monomer emulsion Me1, which is replaced by 135 parts of n-butyl methacrylate. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of the treatment group 1 of this embodiment.

[0120] Treatment Group 4

[0121] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that in step e) of treatment group 1, 10 parts of acrylic acid and 5 parts of itaconic acid are used to prepare the monomer emulsion Me1, and 15 parts of methacrylic acid are used instead. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of treatment group 1 of this embodiment.

[0122] Treatment Group 5

[0123] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between this treatment group and the treatment group 1 is that in the step e) of the treatment group 1, 10 parts of acrylic acid and 5 parts of itaconic acid are used to prepare the monomer emulsion Me1, and 15 parts of acrylic acid are used instead. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of the treatment group 1 of this embodiment.

[0124] Treatment Group 6

[0125] This treatment group refers to the treatment group 1 of this embodiment to prepare the polymer-encapsulated TiO2 composite and its emulsion. The difference between this treatment group and treatment group 1 is that in step e) of treatment group 1, 10 parts of acrylic acid and 5 parts of itaconic acid are used to prepare the monomer emulsion Me1 instead of 10 parts of methacrylic acid and 5 parts of acrylic acid. In addition to the above differences, the materials and process operations used in this treatment group are strictly consistent with those of treatment group 1 of this embodiment.

[0126] Test Example 3

[0127] 1. Test objects: polymer-encapsulated TiO2 composites and their emulsions obtained from treatment groups 1 to 6 of Example 3.

[0128] 2. Test method: The test method refers to the test method performed in Test Example 1.

[0129] 3. Test result analysis:

[0130] The performance test results are shown in Table 4. As can be seen from Table 4, by comparing the performance test results corresponding to treatment group 1 and treatment groups 2 to 6 of Example 3, relative to treatment groups 2 to 6, the polymer-encapsulated TiO2 composite and its emulsion provided by the present invention reasonably arrange the specific components of alkyl methacrylate and carboxyl-containing unsaturated acid in the monomer emulsion Me1 forming the first alkali-swelling coating layer, so that the first alkali-swelling polymer coating layer can form a different refractive index with the second non-alkali-swelling polymer coating layer after adjusting Ph, thereby improving the hiding power of the emulsion.

[0131] Table 4. Performance test results of Example 3

[0132]

[0133] Example 4

[0134] A polymer-encapsulated TiO2 composite and its emulsion, wherein the preparation method comprises the following steps:

[0135] (1) Preparation of dispersant:

[0136] Step a) Preparation of a monomer solution: 14 parts of deionized water, 50 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid, 10 parts of methacryloyloxyethyl trimethylammonium chloride, 15 parts of n-butyl acrylate, 27 parts of methyl methacrylate, 50 parts of anhydrous ethanol, and 2 parts of n-dodecyl mercaptan are weighed according to mass fractions, added into a monomer tank with a stirrer, stirred for 10-15 minutes to mix evenly for later use, to prepare a monomer solution;

[0137] Step b) Add 10 parts of deionized water, 40 parts of anhydrous ethanol, 60 parts of the monomer solution prepared in step a), and 1.3 parts of 2,2-azobis(2,4-dimethylvaleronitrile) to a four-necked flask equipped with a stirrer, a condenser, and a constant flow pump feeding device, and heat the flask until the temperature reaches 55° C., turn off the heating, and allow the system to naturally exotherm and heat up;

[0138] Step c) After the exotherm of step b) reaches a peak value, heating is turned on to keep the system temperature in the four-necked flask at 70° C., and the remaining monomer solution is added for 1 hour; after the monomer solution is added, the temperature is kept at 70° C. for 60 minutes; then the temperature is raised to 77° C., 1.3 parts of 2,2-azobis(2,4-dimethylvaleronitrile) and 2 parts of anhydrous ethanol are added to the flask, and the temperature is kept for another 60 minutes to polymerize the monomer solution to obtain a dispersant polymer;

[0139] Step d) cooling the four-necked flask to room temperature, removing the organic solvent by a rotary evaporator, collecting the dispersant polymer prepared in step c) and drying it, then dissolving the dispersant polymer in water and adding ammonia water to adjust the Ph to 4-6, to prepare a dispersant solution with a Ph of 4-6 and a mass fraction of 21%;

[0140] (2) Preparation of TiO2 slurry:

[0141] Add 72 parts of the above prepared dispersant solution, 240 parts of pure water, and 1000 parts of TiO2 into a steel grinding jar. Slowly add TiO2 while grinding at a speed of 2000 rpm. After adding TiO2, grind the slurry for 20 minutes. The solid content of the slurry is 76.5%.

[0142] (3) Synthesis of TiO2 polymer coating:

[0143] Step e) Preparation of monomer emulsion Me1: according to the mass fractions, 55 parts of pure water, 11 parts of sodium dodecylbenzene sulfonate, 85 parts of methyl methacrylate, 61 parts of n-butyl methacrylate and 14 parts of acrylic acid were weighed and added into an emulsification tank, and mixed evenly for later use;

[0144] Step f) Preparation of monomer emulsion Me2: According to the mass fractions, 100 parts of pure water, 30 parts of sodium lauryl sulfate, 95 parts of n-butyl acrylate, 100 parts of isooctyl acrylate, and 176 parts of styrene are weighed and added into an emulsification tank, and mixed evenly for later use;

[0145] Step g) Add 170 parts of pure water and 1100 parts of the prepared TiO2 slurry into a four-necked flask equipped with a condensing device, a stirring device and a feeding device, and heat the system and maintain it at 50°C;

[0146] Step h) When the temperature of the four-necked flask is maintained at 50° C., the oxidant solution and the reducing agent solution are added dropwise at the same time, and the adding time is 100 min. The monomer emulsion Me1 is added dropwise for 20 min, and the monomer emulsion Me2 is added dropwise for 80 min. Calculated by weight, the oxidant solution includes 11 parts of tert-butyl hydroperoxide and 200 parts of pure water, and the reducing agent solution includes 6 parts of sodium bisulfite and 200 parts of pure water.

[0147] Step i) After the monomer emulsion Me2 is added dropwise, the mixture is kept warm for 60 minutes, then cooled to room temperature and 120 parts by weight of a 5% sodium hydroxide neutralizer is added dropwise within 30 minutes to obtain a polymer-encapsulated composite.

[0148] Step j) 7 parts of titanate coupling agent are added, and the material is filtered to obtain an emulsion formed by a polymer-encapsulated TiO2 composite.

[0149] Example 5

[0150] A polymer-encapsulated TiO2 composite and its emulsion, wherein the preparation method comprises the following steps:

[0151] (1) Preparation of dispersant:

[0152] Step a) Preparation of a monomer solution: 17 parts of deionized water, 30 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid, 12 parts of methacryloyloxyethyl trimethylammonium chloride, 20 parts of isooctyl acrylate, 40 parts of methyl methacrylate, 40 parts of methanol, and 2.5 parts of n-dodecyl mercaptan are weighed according to mass fractions, added into a monomer tank with a stirrer, stirred for 10-15 minutes to mix evenly for later use, to prepare a monomer solution;

[0153] Step b) Add 15 parts of deionized water, 40 parts of methanol, 55 parts of the monomer solution prepared in step a), and 2.5 parts of 2,2-azobis(2,4-dimethylvaleronitrile) to a four-necked flask equipped with a stirrer, a condenser, and a constant flow pump feeding device, and heat the flask until the temperature reaches 55° C., turn off the heating, and allow the system to naturally exotherm and heat up;

[0154] Step c) After the exotherm of step b) reaches a peak value, heating is turned on to keep the system temperature in the four-necked flask at 70° C., and the remaining monomer solution is added for 1 hour; after the monomer solution is added, the temperature is kept at 70° C. for 60 minutes; then the temperature is raised to 77° C., 1.2 parts of 2,2-azobis(2,4-dimethylvaleronitrile) and 3 parts of methanol are added to the flask, and the temperature is kept for another 60 minutes to polymerize the monomer solution to obtain a dispersant polymer;

[0155] Step d) cooling the four-necked flask to room temperature, removing the organic solvent by a rotary evaporator, collecting the dispersant polymer prepared in step c) and drying it, then dissolving the dispersant polymer in water and adding ammonia water to adjust the Ph to 4-6, to prepare a dispersant solution with a Ph of 4-6 and a mass fraction of 21%;

[0156] (2) Preparation of TiO2 slurry:

[0157] Add 72 parts of the above prepared dispersant solution, 240 parts of pure water, and 1000 parts of TiO2 into a steel grinding jar. Slowly add TiO2 while grinding at a speed of 2000 rpm. After adding TiO2, grind the slurry for 20 minutes. The solid content of the slurry is 76.5%.

[0158] (3) Synthesis of TiO2 polymer coating:

[0159] Step e) Preparation of monomer emulsion Me1: according to the mass fractions, 65 parts of pure water, 3 parts of alkyl polyoxyethylene ether, 8 parts of sodium dodecylbenzene sulfonate, 90 parts of methyl methacrylate, 45 parts of hydroxyethyl methacrylate and 20 parts of acrylic acid are weighed and added into an emulsification tank, mixed evenly and set aside;

[0160] Step f) Preparation of monomer emulsion Me2: According to the mass fractions, 100 parts of pure water, 13 parts of alkyl polyoxyethylene ether, 32 parts of sodium lauryl sulfate, 165 parts of n-butyl acrylate, 58 parts of isooctyl acrylate, and 160 parts of styrene are weighed and added into an emulsification tank, mixed evenly and set aside;

[0161] Step g) Add 180 parts of pure water and 980 parts of the prepared TiO2 slurry into a four-necked flask equipped with a condensing device, a stirring device and a feeding device, and heat the system to and maintain it at 50°C;

[0162] Step h) When the temperature of the four-necked flask is maintained at 50° C., the oxidant solution and the reducing agent solution are added dropwise at the same time, and the adding time is 100 min. The monomer emulsion Me1 is added dropwise for 20 min, and the monomer emulsion Me2 is added dropwise for 80 min. Calculated by weight, the oxidant solution includes 11 parts of hydrogen peroxide and 200 parts of pure water, and the reducing agent solution includes 6 parts of isoascorbic acid and 200 parts of pure water.

[0163] Step i) After the monomer emulsion Me2 is added dropwise, the mixture is kept warm for 60 minutes, then cooled to room temperature and 120 parts by weight of a 5% sodium hydroxide neutralizer is added dropwise within 30 minutes to obtain a polymer-encapsulated composite.

[0164] Step j) 7 parts of titanate coupling agent are added, and the material is filtered to obtain an emulsion formed by a polymer-encapsulated TiO2 composite.

[0165] Example 6

[0166] A polymer-encapsulated TiO2 composite and its emulsion, wherein the preparation method comprises the following steps:

[0167] (1) Preparation of dispersant:

[0168] Step a) Preparation of a monomer solution: 14 parts of deionized water, 40 parts of 2-acrylamido-2-methyl-1-propane sulfonic acid, 8 parts of methacryloyloxyethyl trimethylammonium chloride, 10 parts of n-butyl acrylate, 10 parts of isooctyl acrylate, 35 parts of methyl methacrylate, 45 parts of anhydrous ethanol, and 1.5 parts of n-dodecyl mercaptan benzenesulfonate were weighed according to mass fractions, added into a monomer tank with a stirrer, stirred for 10-15 minutes to mix evenly for later use, to prepare a monomer solution;

[0169] Step b) Add 13 parts of deionized water, 35 parts of n-propanol, 55 parts of the monomer solution prepared in step a), and 1.3 parts of 2,2-azobis(2,4-dimethylvaleronitrile) to a four-necked flask equipped with a stirrer, a condenser, and a constant flow pump feeding device, and heat the flask until the temperature reaches 55° C., turn off the heating, and allow the system to naturally exotherm and heat up;

[0170] Step c) After the exotherm of step b) reaches a peak value, heating is turned on to keep the system temperature in the four-necked flask at 70° C., and the remaining monomer solution is added for 1 hour; after the monomer solution is added, the temperature is kept at 70° C. for 60 minutes; then the temperature is raised to 77° C., 1.3 parts of 2,2-azobis(2,4-dimethylvaleronitrile) and 1.3 parts of n-propanol are added to the flask, and the temperature is kept for another 60 minutes to polymerize the monomer solution to obtain a dispersant polymer;

[0171] Step d) cooling the four-necked flask to room temperature, removing the organic solvent by a rotary evaporator, collecting the dispersant polymer prepared in step c) and drying it, then dissolving the dispersant polymer in water and adding ammonia water to adjust the Ph to 4-6, to prepare a dispersant solution with a Ph of 4-6 and a mass fraction of 21%;

[0172] (2) Preparation of TiO2 slurry:

[0173] Add 72 parts of the above prepared dispersant solution, 240 parts of pure water, and 1000 parts of TiO2 into a steel grinding jar. Slowly add TiO2 while grinding at a speed of 2000 rpm. After adding TiO2, grind the slurry for 20 minutes. The solid content of the slurry is 76.5%.

[0174] (3) Synthesis of TiO2 polymer coating:

[0175] Step e) Preparation of monomer emulsion Me1: according to the mass fractions, 60 parts of pure water, 11 parts of sodium dodecylbenzene sulfonate, 62 parts of methyl methacrylate, 85 parts of n-butyl methacrylate, 10 parts of methacrylic acid, and 4 parts of acrylic acid were weighed and added into an emulsification tank, and mixed evenly for later use;

[0176] Step f) Preparation of monomer emulsion Me2: According to the mass fractions, 110 parts of pure water, 10 parts of alkyl polyoxyethylene ether, 35 parts of sodium lauryl sulfate, 185 parts of n-butyl acrylate, 30 parts of isooctyl acrylate, and 170 parts of styrene are weighed and added into an emulsification tank, mixed evenly and set aside;

[0177] Step g) Add 170 parts of pure water and 1100 parts of the prepared TiO2 slurry into a four-necked flask equipped with a condensing device, a stirring device and a feeding device, and heat the system and maintain it at 50°C;

[0178] Step h) When the temperature of the four-necked flask is maintained at 50° C., the oxidant solution and the reducing agent solution are added dropwise at the same time, and the adding time is 100 min. The monomer emulsion Me1 is added dropwise for 20 min, and the monomer emulsion Me2 is added dropwise for 80 min. Calculated by weight, the oxidant solution includes 11 parts of tert-butyl hydroperoxide and 200 parts of pure water, and the reducing agent solution includes 6 parts of isoascorbic acid and 200 parts of pure water.

[0179] Step i) After the monomer emulsion Me2 is added dropwise, the mixture is kept warm for 60 minutes, then cooled to room temperature and 120 parts by weight of a 5% sodium hydroxide neutralizer is added dropwise within 30 minutes to obtain a polymer-encapsulated composite.

[0180] Step j) 8 parts of titanate coupling agent are added, and the material is filtered to obtain an emulsion formed by a polymer-encapsulated TiO2 composite.

[0181] Test Example 4

[0182] 1. Test object: the polymer-encapsulated TiO2 composite and its emulsion obtained in Examples 4 to 6.

[0183] 2. Test method: The test method refers to the test method performed in Test Example 1.

[0184] 3. Test results:

[0185] The performance test results are shown in Table 5.

[0186] Table 5. Performance test results of Examples 4 to 6

[0187]

[0188]

[0189] Comparative Example 1

[0190] This comparative example uses commercially available RS-926W (TiO2 content of 43.4%) as the polymer-encapsulated TiO2 composite and its emulsion.

[0191] Test Example 5

[0192] 1. Test object: the polymer-encapsulated TiO2 composite and its emulsion of Comparative Example 1.

[0193] 2. Test method: The test method refers to the test method performed in Test Example 1.

[0194] 3. Test result analysis:

[0195] The performance test results are shown in Table 6. As can be seen from Table 6, by comparing the performance test results corresponding to the treatment group 1 of Example 1 and the comparative example 1, the emulsion formed by the polymer-encapsulated TiO2 composite provided by the treatment group 1 of Example 1 can achieve a comparable hiding power when the TiO2 content in the emulsion is lower than that in the comparative example 1. Therefore, the polymer-encapsulated TiO2 composite and its emulsion provided by the present invention have excellent hiding performance, can improve the use efficiency, and effectively reduce the amount of TiO2 while ensuring that the hiding power remains unchanged.

[0196] Table 6. Performance test results of comparative example 1

[0197] Test items Comparative Example 1 -5℃ low temperature stability (3 cycles) No abnormality Wet film contrast ratio / % 97.2 Dry film contrast ratio / % 96.1 Washability (number of times) >10000

[0198] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A polymer encapsulated TiO 2 Complex, It is characterized in that The preparation method thereof comprises the following steps: S1. To contain TiO 2 Adding an oxidant solution and a reducing agent solution to an initial reaction solution to obtain a first reaction solution; S2. Adding monomer emulsion Me1 to the first reaction solution to obtain a first mixed solution, polymerizing the monomers contained in the monomer emulsion Me1 to form a first mixed solution. 2 An alkali-swellable polymer coating layer is formed on the surface, wherein the monomer emulsion Me1 contains 100-180 parts of alkyl methacrylate and 10-20 parts of carboxyl-containing unsaturated acid; the alkyl methacrylate S2 is at least one of methyl methacrylate, butyl methacrylate and hydroxyethyl methacrylate; S3. Adding monomer emulsion Me2 to the first mixed solution prepared in S2 to prepare a second mixed solution, polymerizing the monomers contained in the monomer emulsion Me2 to form a second mixed solution. 2 The non-alkali swellable polymer coating layer is formed on the surface of the alkali swellable polymer coating layer, wherein the monomer emulsion Me2 contains 180-250 parts of alkyl acrylate and 120-180 parts of styrene; S4. After cooling to room temperature, a neutralizing agent is added to adjust the Ph of the second mixed solution obtained in S3 to 7.5-8.5, so that the alkali-swellable polymer coating layer and the non-alkali-swellable polymer coating layer swell to different degrees, until the refractive index of the alkali-swellable polymer coating layer is different from the refractive index of the non-alkali-swellable polymer coating layer; The preparation method of the initial reaction solution comprises the following steps: 2 mixing with a dispersant solution and grinding the slurry thus formed; Calculated by weight, the raw materials for preparing the dispersant solution include 35-75 parts of a monomer solution and 1.5-6 parts of an initiator, wherein the monomer solution includes an acrylamide compound, an acrylate compound, a chain transfer agent and an organic solvent.

2. The polymer-encapsulated TiO as claimed in claim 1 2 Complex, It is characterized in that The acrylamide compound includes at least one of 2-acrylamido-2-methyl-1-propane sulfonic acid and methacryloyloxyethyl trimethylammonium chloride; And / or, the acrylic ester compound includes at least one of an acrylic ester monomer and methyl methacrylate, wherein the acrylic ester monomer is selected from at least one of n-butyl acrylate and isooctyl acrylate.

3. The polymer-encapsulated TiO as claimed in claim 1 2 Complex, It is characterized in that The preparation method of the dispersant solution comprises the following steps: Step a, mixing the acrylamide compound, the acrylate compound, the chain transfer agent, and the organic solvent to prepare the monomer solution; Step b, adding the initiator to the monomer solution to cause a polymerization reaction in the monomer solution, and using the polymer obtained after the polymerization reaction as a dispersant polymer; Step c, extracting the dispersant polymer from the product obtained in step b, dissolving the dispersant polymer in water, and the solution thus formed is the dispersant solution.

4. The polymer-encapsulated TiO as claimed in claim 3 2 Complex, It is characterized in that In the process of preparing the dispersant solution, the specific operation of step b includes: first mixing the monomer solution obtained in step a with the initiator and the organic solvent at 70° C., then heating to 77° C. and adding the initiator and the organic solvent for the second time, and keeping the temperature for 60 minutes to obtain the polymer that is the dispersant polymer.

5. The polymer-encapsulated TiO as claimed in claim 3 2 Complex, It is characterized in that In the process of preparing the dispersant solution, the specific operation of step c includes collecting the dispersant polymer obtained in step b, dissolving it in water, and then adding ammonia water to adjust the Ph to 4-6 to obtain the dispersant solution.

6. The polymer-encapsulated TiO as claimed in claim 1 2 Complex, It is characterized in that The carboxyl-containing unsaturated acid in S2 is at least one of methacrylic acid, acrylic acid and itaconic acid.

7. The polymer-encapsulated TiO as claimed in claim 1 2 Complex, It is characterized in that The S3 alkyl acrylate is at least one of n-butyl acrylate and isooctyl acrylate.

8. An emulsion, It is characterized in that The emulsion comprises the polymer-encapsulated TiO 2 The composite, calculated by weight percentage, comprises the polymer-encapsulated TiO 2 TiO in the composite 2 The mass of the emulsion accounts for 32.5±0.5% of the total mass of the emulsion.

9. The emulsion according to claim 8, It is characterized in that The emulsion further comprises a titanate coupling agent. Calculated by mass percentage, the mass of the titanate coupling agent accounts for 0.18-0.35% of the total mass of the emulsion.

Citation Information

Patent Citations

  • Opacifying pigment particle

    CN101891970A

  • Polymer particles

    CN104053729A

  • Opacifying polymer particles

    CN104837933A

  • Method of coating titanium dioxide with polymers

    CN106589204A

  • Polymer-encapsulated pigment particle

    CN107001814A