A non-swelling, high tissue adhesion hydrogel and its preparation method and application in multimodal electrodes

By preparing non-swelling, high tissue adhesion hydrogels and multimodal bioelectrodes, the problem of weak adhesion of bioelectrodes to tissues is solved, and stable integration and signal transmission accuracy on wet dynamic tissue surfaces are achieved, which is suitable for for a variety of biological applications.

CN115975221BActive Publication Date: 2024-10-25HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211619852.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-10-25
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing bioelectrodes have weak adhesion to tissue and cannot be reused, making it difficult to stably integrate on wet dynamic tissue surfaces and affecting the accuracy and stability of signal transmission.

Method used

A non-swelling, highly tissue-adhesive hydrogel was used by grafting chitosan with N-acetyl-L-cysteine, acrylic acid, gelatin, polyvinyl butyral, deionized water and α -Ketoglutaric acid is dissolved in dimethyl sulfoxide and treated with UV irradiation, combined with multi-walled carbon nanotubes and polypyrrole, to prepare a multimodal bioelectrode to achieve long-term stable adhesion and reproducibility.

Benefits of technology

It achieves high tissue adhesion and repeatability on the surface of biological tissues, can accurately monitor electromyographic signals and tissue deformation, and is suitable for applications such as muscle fatigue detection, wound healing, and drug delivery, and the electrodes can be detached on demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115975221B_ABST
    Figure CN115975221B_ABST
Patent Text Reader

Abstract

The present invention discloses a non-swelling, high-tissue-adhesion hydrogel, a preparation method thereof, and an application in a multimodal electrode, and belongs to the technical field of functional composite materials and their preparation. The present invention solves the problems that the existing non-swelling hydrogel has weak adhesion, cannot repair adhesion, cannot be desorbed on demand, and the electrode has no adhesion to wet tissue. The present invention uses chitosan grafted with N-acetyl-L-cysteine, acrylic acid, gelatin, polyvinyl butyral, deionized water, α-ketoglutaric acid, methacrylate gelatin and dimethyl sulfoxide as raw materials to obtain a non-swelling, high-adhesion hydrogel. The present invention also discloses an implantable multimodal bioelectrode, which utilizes a non-swelling dynamic adhesion hydrogel to stably integrate polypyrrole and multi-walled carbon nanotubes on its surface through electrostatic action, so that the multimodal electrode can be stably adhered to the mouse body for a long time, and accurately collect the mouse's electromyographic signals and tissue deformation, and can be desorbed on demand after use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a non-swelling, high-tissue-adhesion hydrogel and a preparation method thereof and application in a multimodal electrode, belonging to the technical field of functional composite materials and preparation thereof. Background Art

[0002] Soft and stretchable bioelectronics that are in close contact with biological tissue interfaces have attracted increasing attention in the scientific community. Bioelectronics can acquire electrophysiological and physical signals (e.g., tissue activity signals of heart rate, body movement, and tissue deformation), which can be used to diagnose and treat various diseases. For example, neural microelectrode arrays (MEAs) that record electroencephalogram (EEG), electromyogram (EMG), and electrocardiogram (ECG) signals from living tissue can be used to diagnose and treat various neurological diseases, such as epilepsy and Parkinson's disease. In addition, stretchable strain sensors can be used to monitor tissue deformation and diagnose movement disorders.

[0003] However, the weak adhesion of existing bioelectrodes to tissues makes it difficult to accurately monitor physiological signals. Although some bioelectrodes that can be adhered to wet dynamic tissues through hydrogel adhesives have been explored, the weak adhesion and high swelling rate of hydrogels to conductive materials will increase the response time of the sensor and reduce the electrical stability and biocompatibility of the device. Although some non-swelling hydrogels have been developed, they exhibit weak tissue adhesion (about 20kPa). This does not ensure the stable integration of electronic devices on wet and dynamic tissue surfaces. At the same time, these hydrogel adhesives form irreversible covalent crosslinks with the tissue surface. When the covalent crosslinks are broken, the adhesion of the hydrogel-tissue interface is permanently and irreversibly lost, so these hydrogel adhesives cannot be reused and exhibit weak adhesion stability. The reusability of hydrogels is essential for adjusting the exact position of electrodes on tissues or repositioning misplaced electrodes. Therefore, the development of non-swelling hydrogels with recoverable tissue adhesion is crucial to improving the accuracy and stability of signal transmission at the bioelectronic-tissue interface. Summary of the invention

[0004] The purpose of the present invention is to solve the problems of weak adhesion of existing non-swelling hydrogels, unrepairable adhesion, inability to desorb on demand, and no adhesion of electrodes to wet tissues, and to provide a hydrogel with low preparation cost, non-swelling, high tissue adhesion, repairable adhesion, and on-demand desorption, and to use it to integrate multi-walled carbon nanotubes and polypyrrole to prepare multimodal bioelectrodes. The electrode has the advantages of wide application, long-term stable adhesion, excellent repeatability, etc., and can effectively broaden the practical application of flexible bioelectronics.

[0005] The technical solution of the present invention:

[0006] One of the purposes of the present invention is to provide a method for preparing a non-swelling, high-tissue-adhesive hydrogel, which comprises: dissolving chitosan grafted with N-acetyl-L-cysteine, acrylic acid, gelatin, polyvinyl butyral, deionized water, α-ketoglutaric acid and methacrylate gelatin in dimethyl sulfoxide, and subjecting the mixture to ultraviolet irradiation treatment to obtain a non-swelling, high-adhesive hydrogel.

[0007] It is further defined that the content of chitosan grafted N-acetyl-L-cysteine ​​is 1-10wt.%, the content of acrylic acid is 10-50wt.%, the content of gelatin is 5-13wt.%, the content of polyvinyl butyral is 1-10wt.%, the content of deionized water is 1-5wt.%, the content of α-ketoglutaric acid is 0.2-1wt.%, and the content of methacrylate gelatin is 0.1-1wt.%.

[0008] It is further defined that the ultraviolet irradiation treatment time is 5 to 20 minutes.

[0009] It is further defined that the preparation process of chitosan grafted N-acetyl-L-cysteine ​​is: disperse chitosan in deionized water, add 1-hydroxybenzotriazole during stirring, continue stirring until the solution is clear, then add N-acetyl-L-cysteine ​​and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, use hydrochloric acid solution to adjust the pH to 4-6, stir at room temperature for 3 hours, then dialyze in deionized water under dark conditions, and freeze-dry the dialyzed fragments to obtain chitosan grafted N-acetyl-L-cysteine.

[0010] It is further defined that the mass of chitosan is 0.1-1 g, the mass of deionized water is 40-50 g, the mass of N-acetyl-L-cysteine ​​is 0.1-0.5 g, and the mass of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 1-3 g.

[0011] Furthermore, the Mw of the dialysis bag is defined as 14,000 to 30,000.

[0012] The second object of the present invention is to provide a method for preparing a multimodal electrode using the non-swelling, high tissue adhesion hydrogel obtained by the above-mentioned preparation method, the method comprising: integrating polypyrrole and multi-walled carbon nanotubes on the surface of the non-swelling, high tissue adhesion hydrogel by drop coating, photolithography, transfer and pre-stretching to obtain a multimodal electrode.

[0013] It is further defined that the specific operation process of the method is: dropping a multi-walled carbon nanotube solution on the surface of the hydrogel, evaporating the solvent to form a strain sensor, and then pre-stretching the strain sensor and covering it on glass containing a polypyrrole electrode to obtain a multimodal electrode.

[0014] It is further defined that the pre-stretching strain is 30% to 100%.

[0015] It is further defined that the amount of the multi-walled carbon nanotube solution is 50 to 1000 μL, and the concentration of the multi-walled carbon nanotube solution is 2 to 10 mg / mL.

[0016] It is further defined that the preparation method of the glass containing the polypyrrole electrode is:

[0017] First, a layer of photoresist is spin-coated on the conductive glass, and the electrode pattern is prepared by photolithography;

[0018] Then, polypyrrole electrodes were synthesized by electroplating on conductive glass via pyrrole anodization.

[0019] Further, the process of electroplating the polypyrrole electrode on the conductive glass is as follows: dissolve the pyrrole monomer and p-toluenesulfonic acid monohydrate in 30-100 ml of water, use a Keithley 2450 digital source meter set at 0.5-8 mA / cm 2 After the polymerization reaction at a constant current density of 10 to 50 minutes, polypyrrole was synthesized, and then a layer of photoresist was spin-coated on the polypyrrole to encapsulate the polypyrrole to obtain glass containing polypyrrole electrodes.

[0020] It is further defined that the mass of the pyrrole monomer is 0.1 to 0.5 g, and the mass of the p-toluenesulfonic acid monohydrate is 1 to 5 g.

[0021] It is further limited that the photolithography time is 1 to 20 seconds.

[0022] The third object of the present invention is to provide a multimodal electrode obtained by the above-mentioned preparation method, which is specifically used for the preparation of bioelectronics, epidermal physiological signal monitoring, epidermal muscle fatigue monitoring, rat subcutaneous muscle physiological signal monitoring, muscle fatigue monitoring, wound healing, drug delivery or artificial prosthesis control.

[0023] Further specifically, the multimodal electrode can be repeatedly peeled from the biological tissue using a desorption solution.

[0024] It is further defined that the content of sodium chloride in the desorption solution is 1-25 wt.%, and the mass of reduced glutathione is 1-10 wt.%.

[0025] Compared with the prior art, this application has the following beneficial effects:

[0026] (1) The present invention aims to solve the problems that non-swelling hydrogels exhibit weak tissue adhesion and these hydrogel adhesives form irreversible covalent crosslinks with the tissue surface. Hydrophobic polyvinyl butyral and dynamic bonds are introduced to achieve non-swelling and dynamic bond adhesion, and can be desorbed on demand. Multimodal bioelectrodes are constructed based on this hydrogel for monitoring electromyographic signals and tissue deformation on the body surface and in the body. They can be used in many fields such as muscle fatigue detection, wound healing, drug delivery, and artificial prosthesis manipulation.

[0027] (2) The non-swelling dynamic adhesion hydrogel provided by the present invention can stably integrate polypyrrole and multi-walled carbon nanotubes on its surface through electrostatic action, so that the multimodal electrode can be stably adhered to the mouse body for a long time and accurately collect the mouse's electromyographic signals and tissue deformation, and can be desorbed on demand after use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The time-swelling rate curves of different types of hydrogels;

[0029] Figure 2 The adhesion strength of the hydrogel prepared in Example 1 after different number of cycles of adhesion;

[0030] Figure 3 Effects of the electrode prepared in Example 1 with and without a desorption solution on tissue adhesion;

[0031] Figure 4 Collect epidermal EMG signals and tissue deformation maps for different types of multimodal electrodes;

[0032] Figure 5 To judge whether the muscle is in fatigue state through electromyographic signal and tissue deformation;

[0033] Figure 6 Photo of a multimodal electrode implanted in the subcutaneous muscle of a mouse;

[0034] Figure 7 Use multimodal electrodes to collect EMG signals and tissue deformation of subcutaneous muscles of mice;

[0035] Figure 8 To judge whether the muscle is in a state of fatigue through electromyographic signals and tissue deformation. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0037] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0038] Embodiment 1:

[0039] This embodiment provides a method for preparing a non-swelling, high tissue adhesion hydrogel, the method comprising the following steps:

[0040] Step 1: Preparation of chitosan grafted with N-acetyl-L-cysteine:

[0041] 0.9 g of chitosan was dispersed in 50 g of deionized water, and 0.4 g of 1-hydroxybenzotriazole was added to the above suspension while stirring until a clear solution was obtained, 0.4 g of N-acetyl-L-cysteine ​​and 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride were added to the solution, and the pH of the mixed solution was adjusted to 6 using 1 mol / L hydrochloric acid, then stirred and incubated at room temperature for 3 h, then placed in the dark, dialyzed in deionized water, and then the dialyzed fragments were freeze-dried and stored.

[0042] Step 2: Preparation of non-swelling, highly adhesive hydrogel:

[0043] Chitosan grafted N-acetyl-L-cysteine, acrylic acid, gelatin, polyvinyl butyral, deionized water, α-ketoglutaric acid and methacrylate gelatin are dissolved in dimethyl sulfoxide, wherein the chitosan grafted N-acetyl-L-cysteine ​​content is 1wt.%, the acrylic acid content is 10wt.%, the gelatin content is 6wt.%, the polyvinyl butyral content is 2wt.%, the deionized water content is 5wt%, the α-ketoglutaric acid content is 0.2wt.%, and the methacrylate gelatin content is 1wt.%. The mixed solution is irradiated with ultraviolet light for 10 minutes to obtain a non-swelling, high-adhesion hydrogel.

[0044] Step 3: Prepare strain sensor:

[0045] First, sodium chloride and reduced glutathione are dissolved in deionized water to obtain a desorption solution, wherein the content of sodium chloride is 20wt.%, and the mass of reduced glutathione is 5wt.%;

[0046] Then, 60 μL of a 3 mg / mL multi-walled carbon nanotube solution was dropped on the surface of the non-swelling hydrogel, and the strain sensor was formed after the solvent evaporated. The multi-walled carbon nanotube solution was dropped on the surface of the hydrogel, and the strain sensor was formed after the solvent evaporated. The strain sensor was pre-stretched and covered on the glass containing the polypyrrole electrode to obtain a multimodal electrode.

[0047] The preparation method of glass containing polypyrrole electrode is as follows: first, a layer of photoresist is spin-coated on the conductive glass, and an electrode pattern is prepared by photolithography for 20 seconds; then, 0.5g of pyrrole monomer and 5g of p-toluenesulfonic acid monohydrate are dissolved in 100ml of water, and a Keithley 2450 digital source meter is used to set 0.5mA / cm 2 After 50 minutes of polymerization reaction at a constant current density, polypyrrole was synthesized, and a layer of photoresist was spin-coated on the polypyrrole to encapsulate the polypyrrole, thereby obtaining glass containing polypyrrole electrodes. The pre-stretching strain of the strain sensor was 100%.

[0048] Comparative Example 1:

[0049] The difference between this comparative example and Example 1 is that polyvinyl butyral is not added in step 2, and the remaining process steps and parameter settings are the same as those in Example 1.

[0050] Effect example:

[0051] (1) The swelling ratio of the hydrogels obtained in Example 1 and Comparative Example 1 was characterized by soaking a hydrogel with a length of 1 cm, a width of 1 cm, and a thickness of 1 mm in a phosphate buffer solution. After soaking for different periods of time, the dimensions of the hydrogels were collected and the volume was calculated as V. The initial volume was V0, and the swelling ratio was V / V0. The results are shown in FIG. Figure 1 As shown by Figure 1 It can be seen that the swelling ratio of the hydrogel obtained in Example 1 is only 1.2, which is almost negligible, while the swelling ratio of Comparative Example 1 reaches 45, indicating that the hydrogel obtained in Example 1 exhibits non-swelling characteristics.

[0052] (2) The adhesion strength of the hydrogel obtained in Example 1 was characterized by measuring the adhesion strength by an overlap shear test on an electronic universal testing machine. The sample sizes were 2 cm (width) and 4 cm (length). The overlap area was 2 cm -2 . One hour after the overlap is completed, the adhesion strength is measured. The adhesion strength is calculated by dividing the force by the peeled area. At least 4 samples are tested under each condition. The results are shown in Figure 2 As shown, Figure 2 It can be seen that after the hydrogel obtained in Example 1 was cyclically adhered for 8 times (desorbed using a desorption solution), it still had an adhesion force of 70 kPa to the tissue, indicating that the hydrogel had recoverable adhesion.

[0053] The adhesion strength of the electrode obtained in Example 1 was characterized by measuring the adhesion strength by an overlap shear test on an electronic universal testing machine. The sample sizes were 2 cm (width) and 4 cm (length). The overlap area was 2 cm -2. One hour after the lap joint was completed, the adhesion strength was measured. The adhesion strength without the use of the desorption solution was calculated by dividing the force by the peeled area. At least 4 samples were tested under each condition. The results are shown in Figure 3 As shown in “No desorption solution”.

[0054] The adhesion strength after using the desorption solution was measured by lap shear test on an electronic universal testing machine. The sample dimensions were 2 cm (width) and 4 cm (length). The lap area was 2 cm -2 After 1 hour, soak the samples in the desorption solution for 10 minutes. Measure the adhesion strength and divide the force by the peeled area to calculate the adhesion strength after using the desorption solution. At least 4 samples were tested under each condition. The results are shown in Figure 3 As shown in “with desorption solution”, by comparison, the adhesion strength decreases rapidly after using the desorption solution, indicating that this hydrogel can achieve on-demand benign desorption after using the desorption solution.

[0055] (3) The electrodes obtained in Example 1 and existing commercial electrodes were used to detect epidermal electromyographic signals and tissue deformation. The detection conditions were as follows: the electrodes were attached to the palmaris longus muscle of the arm, the electromyographic signals and tissue deformation were recorded by an electrophysiological signal collector and a digital source meter, and the counter electrode and reference electrode were attached to the wrist. The results are shown in Figure 2. Figure 4 As shown, Figure 4 a is the epidermal electromyographic signal, Figure 4 a It can be seen that the quality of the collected EMG signals is comparable to that of commercial electrodes; Figure 4 b is the tissue deformation signal obtained by the electrode provided in Example 1, Figure 4 It can be seen that it can accurately detect the deformation signal of the tissue.

[0056] (4) Attach the electrodes to the subcutaneous muscles of the rats, such as Figure 6 As shown, the electromyographic signals and tissue deformation were recorded by an electrophysiological signal collector and a digital source meter, and the counter electrode and the reference electrode were attached to the upper and lower sides of the rat's legs. Figure 7 The multimodal electrode simultaneously and accurately collects the subcutaneous electromyographic signals and tissue deformation signal images of rats.

[0057] (5) Figure 5 For Figure 4 Obtain data and calculate and curve fit results through MATLAB software, such as Figure 5 It can be seen that the electrode can realize accurate muscle fatigue detection and the muscle is in a fatigue state.

[0058] Figure 8 against Figure 7 Obtain data and calculate and curve fit results through MATLAB software, such as Figure 8 It can be seen that the electrode can realize accurate muscle fatigue detection and the muscle is in a fatigue state.

[0059] Although the present invention has been disclosed as above in the preferred embodiments, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a non-swelling, high tissue adhesion hydrogel, characterized in that: Chitosan grafted with N-acetyl-L-cysteine, acrylic acid, gelatin, polyvinyl butyral, deionized water, α-ketoglutaric acid and methacrylate gelatin were dissolved in dimethyl sulfoxide and treated with ultraviolet irradiation to obtain a non-swelling, high-adhesion hydrogel; The chitosan grafted N-acetyl-L-cysteine ​​content is 1-10wt.%, the acrylic acid content is 10-50wt.%, the gelatin content is 5-13wt.%, the polyvinyl butyral content is 1-10wt.%, the deionized water content is 1-5wt.%, the α-ketoglutaric acid content is 0.2-1wt.%, and the methacrylate gelatin content is 0.1-1wt.%; The preparation process of chitosan grafted N-acetyl-L-cysteine ​​is as follows: dispersing chitosan in deionized water, adding 1-hydroxybenzotriazole during stirring, continuing stirring until the solution is clear, then adding N-acetyl-L-cysteine ​​and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, adjusting the pH to 4-6 with a hydrochloric acid solution, stirring at room temperature for 3 hours, then dialyzing in deionized water under dark conditions, and freeze-drying the dialyzed fragments to obtain chitosan grafted N-acetyl-L-cysteine.

2. The method for preparing the non-swelling, high tissue adhesion hydrogel according to claim 1, characterized in that: The ultraviolet irradiation treatment time is 5 to 20 minutes.

3. A non-swelling, high tissue adhesion hydrogel, characterized in that: The method is obtained by the preparation method described in any one of claims 1 to 2.

4. A method for preparing a multimodal electrode, characterized in that: Polypyrrole and multi-walled carbon nanotubes are integrated on the surface of the non-swelling, high tissue adhesion hydrogel of claim 3 by drop coating, photolithography, transfer and pre-stretching to obtain a multimodal electrode.

5. The method for preparing a multimodal electrode according to claim 4, characterized in that: A multi-walled carbon nanotube solution is dropped onto the surface of the hydrogel, and the solvent evaporates to form a strain sensor, which is pre-stretched and covered on glass containing a polypyrrole electrode to obtain a multimodal electrode; the pre-stretching strain is 30% to 100%.

6. A multimodal electrode, characterized in that: The method is obtained by the preparation method described in claim 4 or 5.

Citation Information

Patent Citations

  • Staged acting antibacterial hydrogel dressing and preparation method thereof

    CN104225668A

  • Preparation method and application of conductive gel material

    CN113896909A

  • Temperature-sensitive debonding wet tissue adhesion hydrogel and preparation method thereof

    CN114644766A

  • Application of hydrogel in preparation of highly bionic artificial blood vessel material

    CN115212350A

  • Biomedical electrode

    JP2022012318A