Acetylene carbon black pelletizing method and system
By preheating the acetylene carbon black to 0.8 to 1.2 times the temperature of the infiltration water, and granulating it in the infiltration water of 50°C to 95°C, the problem of low yield of acetylene carbon black in the existing technology is solved, and the acetylene production rate is improved. Carbon black yield and particle size uniformity.
Patent Information
- Application Number
- CN202310009162.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-04
AI Technical Summary
In the prior art, only 80°C pure water is used as the infiltration water, resulting in a too low yield of qualified particle size of acetylene carbon black.
By preheating acetylene carbon black, the preheating temperature is set to 0.8 to 1.2 times the temperature of the infiltration water, and the infiltration and granulation are performed within the temperature range of the infiltration water of 50°C to 95°C, followed by drying to improve the quality of acetylene carbon black. yield and particle size uniformity.
The yield of acetylene carbon black is increased, the yield of qualified particle size is increased by 3% to 10% on average, and the loss rate of carbon black is reduced.
Smart Images

Figure CN115975404B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon black granulation, and in particular to an acetylene carbon black granulation method and system. Background Art
[0002] Acetylene black (also known as acetylene black) is a carbon black obtained by continuous pyrolysis of acetylene with a purity of more than 99% obtained by decomposition and refining of by-product gas during the pyrolysis of calcium carbide or naphtha (raw gasoline). Compared with furnace carbon black, its crystallization and secondary structure are more developed, so its conductivity and liquid absorption are also better. Due to the small amount of impurities such as heavy metals, the loss caused by self-discharge is small. It is mainly used for the negative electrode of nickel-hydrogen batteries, and can also be used in supercapacitors as a conductor.
[0003] In order to facilitate transportation and improve the comprehensive performance of acetylene carbon black, so that acetylene carbon black can be widely used in new lead-acid batteries, primary and secondary lithium batteries and ultra-high voltage cables and other fields, acetylene carbon black needs to be granulated. Due to the high structure of acetylene carbon black, the dry granulation process is difficult to achieve. The wet granulation process is currently the main technology for acetylene carbon black granulation. For example, the Chinese invention patent with publication number CN104371380A discloses a method for wet granulation of carbon black and a manufacturing system for wet granulation of carbon black, and specifically discloses that the carbon black powder material output by the quantitative feeder continuously enters the high-speed stirring tooth granulator, and is fully contacted with the binder input by the binder supply system in the granulator to achieve mixing, granulation, spheroidization, densification and other processes.
[0004] Although the above-mentioned carbon black wet granulation method and a carbon black wet granulation manufacturing system have preliminarily achieved the granulation of acetylene carbon black, during the granulation process, honey or wood cellulose is added as a binder, which indirectly introduces impurities, affects the purity of acetylene carbon black, and cannot meet the requirements of some products.
[0005] In order to solve the above technical problems, the Chinese invention patent with publication number CN110437650A discloses a granular conductive carbon black and a preparation method thereof, wherein the conductive carbon black raw material is first wetted with water at a temperature ≥ 80°C to enhance the hydrophilicity of the conductive carbon black raw material, and then granulated conductive acetylene carbon black with uniform particle size distribution is obtained by wet granulation and drying. Furthermore, the conductive carbon black raw material and water vapor or water are introduced into an impregnation device for impregnation, while nitrogen is introduced to balance the pressure in the impregnation device, and then the conductive carbon black raw material wetted with water vapor or water is transported to a wet granulator, and deionized water is added for wet granulation.
[0006] In the above-mentioned acetylene carbon black granulation method and system, the wetting medium is water, and pure water with a temperature ≥80°C is used as the wetting water to improve the strength uniformity of the acetylene carbon black. However, in actual practice, only pure water with a temperature of 80°C is used as the wetting water, and the yield of granular acetylene carbon black with a qualified particle size is too low. Summary of the invention
[0007] Based on this, the present invention provides an acetylene black granulation method and system to solve the technical problem in the prior art that only 80° C. pure water is used as the wetting water, resulting in too low a yield of granular acetylene black with a qualified particle size.
[0008] The technical solution of the present invention to solve the above technical problems is as follows:
[0009] An acetylene carbon black granulation method, characterized in that it comprises the following steps:
[0010] a. Feeding acetylene black and preheating the acetylene black;
[0011] b. Adding soaking water to the acetylene black feed for soaking, the soaking water temperature is 50 ℃ ~ 95 ℃;
[0012] c. granulating the impregnated acetylene carbon black to form granular acetylene carbon black;
[0013] d. drying the granulated acetylene carbon black to obtain an acetylene carbon black product;
[0014] In step a, the feed temperature of acetylene black is preheated to 0.8 to 1.2 times the temperature of the soaking water.
[0015] Preferably, the preheating temperature is preheated to a temperature difference of ±1°C from the temperature of the soaking water.
[0016] Preferably, the temperature of the soaking water used is 50°C to 80°C.
[0017] An acetylene carbon black granulation system, comprising:
[0018] A preheating device, used for preheating acetylene carbon black feed;
[0019] An impregnation device, connected to the preheating device, the impregnation device is connected to an impregnation water feed pipe and is used to impregnate the acetylene carbon black;
[0020] a granulation device, connected to the impregnation device, for granulating the impregnated acetylene carbon black; and
[0021] A drying device is connected to the granulating device and is used to dry the granulated acetylene black.
[0022] Preferably, the discharge end of the preheating device is provided with a carbon black temperature detection device, which is used to detect the temperature of acetylene black at the discharge end of the preheating device, and the wetting water feed pipe is provided with a wetting water temperature detection device, which is used to detect the temperature of the wetting water; the preheating device is also provided with a first jacket, the first jacket is provided with a first medium-temperature gas feed pipe, the first medium-temperature gas feed pipe is provided with a medium-temperature gas feed flow regulating valve, and the medium-temperature gas feed flow regulating valve regulates the flow of the medium-temperature gas feed flow regulating valve according to the temperature difference fed back by the carbon black temperature detection device and the wetting water temperature detection device, so that the temperature difference between the detection temperature of the carbon black temperature detection device and the detection temperature of the wetting water temperature detection device is within the process range.
[0023] Preferably, the drying device further comprises a drying drum and a hot air generator, a heating chamber is arranged outside the drying drum, and the drying drum can rotate in the heating chamber. The hot air generator is provided with a hot gas discharge pipe, and the hot gas discharge pipe is connected to the feed end of the heating chamber.
[0024] Preferably, the hot gas discharge pipe is connected to the first medium-temperature gas feed pipe.
[0025] Preferably, the first medium-temperature gas feed pipe is connected to the drying device discharge pipe.
[0026] Preferably, the hot gas discharge pipe is provided with a first flow regulating valve, the drying device discharge pipe is provided with a second flow regulating valve, and the first medium-temperature gas feed pipe is provided with a temperature sensor for detecting the temperature of the first medium-temperature gas feed pipe. The first flow regulating valve and the second flow regulating valve adjust the gas flow of the first medium-temperature gas feed pipe and the drying device discharge pipe according to the temperature feedback from the temperature sensor.
[0027] Preferably, the preheating device is arranged at the front end of the infiltration device, and the preheating device and the infiltration device also include a conveying shaft running through the preheating device and the infiltration device, and the conveying shaft is provided with a spiral conveying plate at one end of the preheating device, and the conveying shaft is provided with rake teeth at one end of the infiltration device.
[0028] Compared with the prior art, the present invention has at least the following advantages:
[0029] The acetylene carbon black granulation method provided by the present invention preheats the acetylene carbon black feed. The method comprises the following steps: firstly preheating the acetylene carbon black until the feed temperature of the acetylene carbon black is 0.8 to 1.2 times the temperature of the soaking water. Experiments show that preheating the acetylene carbon black to a temperature close to that of the soaking water is beneficial to improving the yield of the acetylene carbon black. The yield of the acetylene carbon black with a qualified particle size is increased by 3% to 10% on average.
[0030] The present invention also provides an acetylene carbon black granulation system, which realizes preheating of acetylene carbon black through a preheating device, an impregnation device, a granulation device and a drying device, and then the preheated acetylene carbon black enters the impregnation device and is impregnated with impregnation water, and then the impregnated acetylene carbon black enters the granulation device and is granulated to obtain granular acetylene carbon black, and then the granulated acetylene carbon black enters the drying device and is dried to obtain an acetylene carbon black product; since the acetylene carbon black is first preheated to a temperature close to that of the impregnation water, the yield of granular acetylene carbon black with a target particle size is increased and the loss rate of carbon black is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the structure of an acetylene carbon black granulation method and system
[0032] In the figure: acetylene carbon black granulation system 10, carbon black temperature detection device 100, first jacket 110, first medium-temperature gas feed pipe 120, medium-temperature gas feed flow regulating valve 121, temperature sensor 130, conveying shaft 140, spiral conveying plate 150, wetting water feed pipe 200, wetting water temperature detection device 210, rake teeth 220, drying drum 300, heating chamber 310, hot air generator 320, hot gas feed pipe 330, first flow regulating valve 331, drying device discharge pipe 340, second flow regulating valve 341. DETAILED DESCRIPTION
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0034] In a specific embodiment of the present invention, a method for granulating acetylene carbon black comprises the following steps:
[0035] a. Feeding acetylene black and preheating the acetylene black;
[0036] Preferably, acetylene carbon black with a carbon black oil absorption value of ≥220 ml / L and an iodine adsorption capacity of 60 to 100 mg / g is used as a raw material, and the acetylene carbon black is first preheated to 0.8 to 1.2 times the temperature of the soaking water. For example, when the determined soaking water process temperature is too high, the preheating temperature is reduced, and when the determined soaking water process temperature is too low, the preheating temperature is increased.
[0037] b. Adding soaking water to the acetylene black feed for soaking, the soaking water temperature is 50 ℃ ~ 95 ℃;
[0038] Preferably, the preheated acetylene carbon black is conveyed to an impregnation device, the impregnation water is pure water at 50°C to 95°C, and the amount of impregnation water and the amount of acetylene carbon black are introduced into the impregnation device at a mass ratio of 3:1 to 2:1 for impregnation. The acetylene carbon black and the impregnation water are fully contacted and mixed by sufficient stirring to improve the hydrophilicity of the acetylene carbon black.
[0039] c. granulating the impregnated acetylene carbon black to form granular acetylene carbon black;
[0040] Preferably, the acetylene carbon black after impregnation is transported to a granulation device, which is provided with a rake tooth 220 granulator, and granulation water is added into the rake tooth 220 granulator through the rake tooth 220 granulator. Preferably, the temperature of the granulation water is 60° C. to 85° C., and the amount of granulation water and the amount of acetylene carbon black are introduced into the granulation device in a mass ratio of 6:3 to 5:3, and the acetylene carbon black is granulated. The acetylene carbon black is fully contacted with the granulation water to achieve mixing, granulation, spheroidization, densification and other processes to obtain granulated acetylene carbon black.
[0041] d. Drying the granulated acetylene black to obtain an acetylene black product.
[0042] Preferably, the granulated acetylene carbon black is transported to a drying device for drying. The temperature of the drying device is 160°C to 310°C. After the granulated acetylene carbon black is dried and screened, a granulated acetylene carbon black product is obtained.
[0043] In a preferred embodiment, the preheating temperature is preheated to a temperature difference of ±1°C from the temperature of the soaking water.
[0044] The acetylene carbon black is first preheated to a temperature close to that of the soaking water, thereby increasing the yield of granular acetylene carbon black with a target particle size and reducing the loss rate of carbon black.
[0045] In a preferred embodiment, the temperature of the soaking water is 50°C to 80°C.
[0046] The infiltration water is pure water at 50°C to 80°C. The infiltration water is passed into the infiltration device for infiltration. The acetylene carbon black is fully contacted and mixed with the infiltration water by sufficient stirring to improve the hydrophilicity of the acetylene carbon black. Compared with the prior art, the preheating method can effectively reduce the temperature of the infiltration water while ensuring the uniform particle size of the acetylene carbon black.
[0047] An acetylene carbon black pelletizing system, please refer to Figure 1 ,include:
[0048] A preheating device, used for preheating acetylene carbon black feed;
[0049] The impregnation device is connected to the preheating device, and the impregnation device is connected to an impregnation water feed pipe 200 for impregnating acetylene carbon black.
[0050] a granulation device, connected to the impregnation device, for granulating the impregnated acetylene carbon black; and
[0051] A drying device is connected to the granulating device and is used to dry the granulated acetylene black.
[0052] The acetylene carbon black granulation method provided by the present invention comprises the following steps: the acetylene carbon black enters a preheating device, and the method comprises the following steps: firstly, preheating the acetylene carbon black feed material until the feed temperature of the acetylene carbon black is 0.8 to 1.2 times the temperature of the soaking water. Experiments show that preheating the acetylene carbon black to a temperature close to that of the soaking water is beneficial to improving the yield of the acetylene carbon black, and the yield of the acetylene carbon black with a qualified particle size is increased by 3% to 10% on average.
[0053] The present invention also includes an acetylene carbon black granulation system, which includes a preheating device, an impregnation device, a granulation device and a drying device. The acetylene carbon black is first transported to the preheating device to preliminarily preheat the acetylene carbon black. The acetylene carbon black after preliminarily preheating is transported to the impregnation device, and a certain amount of impregnation water is added to the impregnation section to impregnate the acetylene carbon black. The impregnated acetylene carbon black is granulated by the granulation device to obtain granular acetylene carbon black. The granulated acetylene carbon black is transported to the drying device for drying to obtain an acetylene carbon black product. Experiments show that preheating the acetylene carbon black to a temperature close to that of the impregnation water is beneficial to improving the yield of the acetylene carbon black during the acetylene carbon black granulation process.
[0054] In a preferred embodiment, the discharge end of the preheating device is provided with a carbon black temperature detection device 100, which is used to detect the temperature of acetylene carbon black at the discharge end of the preheating device, and the soaking water feed pipe 200 is provided with a soaking water temperature detection device 210, which is used to detect the temperature of soaking water. The preheating device is provided with a first jacket 110, and the first jacket 110 is provided with a first medium-temperature gas feed pipe 120, and the first medium-temperature gas feed pipe 120 is provided with a medium-temperature gas feed flow regulating valve 121, and the medium-temperature gas feed flow regulating valve 121 regulates the flow difference of the medium-temperature gas feed flow regulating valve 121 according to the temperature feedback from the carbon black temperature detection device 100 and the soaking water temperature detection device 210, so that the temperature difference between the detection temperature of the carbon black temperature detection device 100 and the detection temperature of the soaking water temperature detection device 210 is within the process range.
[0055] The carbon black temperature detection device 100 detects and feeds back the temperature of acetylene carbon black according to the set process temperature of the discharge end of the preheating device; the soaking water temperature detection device 210 detects and feeds back the temperature of soaking water according to the set process temperature of soaking water. The medium-temperature gas feed flow control valve 121 adjusts the process temperature according to the process temperature of the discharge end of the preheating device and the process temperature of soaking water. For example, when the carbon black temperature detection device 100 and the soaking water temperature detection device 210 detect and feed back the temperature of the discharge end of the preheating device and the temperature of soaking water greater than the set temperature of the discharge end of the preheating device and the temperature of soaking water, the flow of the medium-temperature gas feed flow control valve 121 is reduced; when the carbon black temperature detection device 100 and the soaking water temperature detection device 210 detect and feed back the temperature of the discharge end of the preheating device and the temperature of soaking water less than the set temperature of the discharge end of the preheating device and the temperature of soaking water, the flow of the medium-temperature gas feed flow control valve 121 is increased. Therefore, the acetylene carbon black is first preheated to a temperature close to that of the soaking water, which is beneficial to increasing the yield of granular acetylene carbon black of target particle size and reducing the loss rate of acetylene carbon black.
[0056] In a preferred embodiment, the drying device further includes a drying drum 300 and a hot air generator 320. The drying device includes a drying drum 300, a heating chamber 310 is arranged outside the drying drum 300, and the drying drum 300 can rotate in the heating chamber 310. The hot air generator 320 is provided with a first hot gas discharge pipe, and the hot gas discharge pipe is connected to the feed end of the heating chamber 310.
[0057] The hot gas generated by the hot air generator 320 is introduced into the heating chamber 310 to exchange heat with the granular acetylene carbon black in the drying drum 300 to reduce the moisture content of the granular acetylene carbon black. The heating chamber 310 is heated, and the hot gas is introduced into the drying device for heating. After heat exchange with the granular acetylene carbon black, the remaining tail gas energy still has a high residual temperature. This part of the energy is used as a heat source for recycling and utilization, effectively reducing energy consumption.
[0058] In a preferred embodiment, the hot gas discharge pipe is connected to the first medium-temperature gas feed pipe 120 .
[0059] The hot gas discharge pipe is connected to the first medium-temperature gas feed pipe 120, so that the hot gas in the hot gas feed pipe 330 flows to the first medium-temperature gas feed pipe 120, and hot gas is introduced into the first medium-temperature gas feed pipe 120 to provide a heat source for the preheating device.
[0060] In a preferred embodiment, the first medium-temperature gas feed pipe 120 is connected to the drying device discharge pipe 340 .
[0061] The first medium-temperature gas feed pipe 120 is connected to the drying device, and the tail gas cold gas of the drying device is introduced into the first medium-temperature gas feed pipe 120, so that the temperature of the preheating device is controlled within a set range.
[0062] In a preferred embodiment, the hot gas discharge pipe is provided with a first flow regulating valve 331, the drying device discharge pipe 340 is provided with a second flow regulating valve 341, and the first medium-temperature gas feed pipe 120 is provided with a temperature sensor 130 for detecting the temperature of the first medium-temperature gas feed pipe 120. The first flow regulating valve 331 and the second flow regulating valve 341 adjust the gas flow in the first medium-temperature gas feed pipe 120 and the drying device discharge pipe 340 according to the temperature feedback from the temperature sensor 130.
[0063] The process temperature is adjusted according to the set process temperature of the first medium-temperature gas feed pipe 120. For example, when the temperature sensor 130 detects and feedbacks that the temperature of the first medium-temperature gas feed pipe 120 is lower than the set temperature, the first flow regulating valve 331 on the hot gas discharge pipe is opened, and the second flow regulating valve 331 on the drying device discharge pipe 340 is closed; when the temperature sensor 130 detects and feedbacks that the temperature of the first medium-temperature gas feed pipe 120 is higher than the set temperature, the first flow regulating valve 331 on the hot gas discharge pipe is closed, and the second flow regulating valve 331 on the drying device discharge pipe 340 is opened.
[0064] In a preferred embodiment, the preheating device is arranged at the front end of the infiltration device, and the preheating device and the infiltration device also include a conveying shaft 140 that runs through the preheating device and the infiltration device, and the conveying shaft 140 is located at one end of the preheating device and is provided with a spiral conveying plate 150, and the conveying shaft 140 is located at one end of the infiltration device and is provided with rake teeth 220.
[0065] Through the conveying device running through the preheating section and the impregnation device, the acetylene carbon black first enters the preheating device for preliminary preheating and then is conveyed to the impregnation device. The impregnation water is introduced through the impregnation water feed pipe 200 to impregnate the acetylene carbon black. The acetylene carbon black is first preheated to a temperature close to that of the impregnation water, so that the granulation is more uniform and the yield of the acetylene carbon black is improved.
[0066] The technical features and effects of the present invention are further illustrated below through specific experimental examples.
[0067] Experimental Example 1
[0068] First, the acetylene carbon black is preheated to room temperature, 40°C, 65°C, 96°C and 80°C respectively. The acetylene carbon black enters the impregnation device, the temperature of the impregnation water is 80°C, and the impregnation water is sprayed into the acetylene carbon black for impregnation. The acetylene carbon black after impregnation enters the granulation device, the temperature of the granulation water is 75°C, and the granulation device is provided with a rake tooth 220 granulator. Granular acetylene carbon black is sprayed with granulation water for granulation. Granular acetylene carbon black is obtained after granulation. The granulated acetylene carbon black after granulation enters the drying device, and the drying temperature is 280°C. The granulated acetylene carbon black is sieved and tested, and the loss rate of acetylene carbon black is calculated.
[0069]
[0070]
[0071] Experimental Example 2
[0072] First, the acetylene carbon black is preheated to room temperature and 60°C respectively. The acetylene carbon black enters the impregnation device, the temperature of the impregnation water is 50°C, and the impregnation water is sprayed on the acetylene carbon black for impregnation. The acetylene carbon black after impregnation enters the granulation device, the temperature of the granulation water is 75°C, and the granulation device is provided with a rake tooth 220 granulator. Granular acetylene carbon black is sprayed with granulation water for granulation. Granular acetylene carbon black is obtained after granulation. The granulated acetylene carbon black after granulation enters the drying device, and the drying temperature is 280°C. The granulated acetylene carbon black is sieved and tested, and the loss rate of acetylene carbon black is calculated.
[0073] Experimental Example 3
[0074] First, the acetylene carbon black is preheated to room temperature and 80°C respectively. The acetylene carbon black enters the impregnation device, the temperature of the impregnation water is 95°C, and the impregnation water is sprayed on the acetylene carbon black for impregnation. The acetylene carbon black after impregnation enters the granulation device, the temperature of the granulation water is 75°C, and the granulation device is provided with a rake tooth 220 granulator. Granular acetylene carbon black is sprayed with granulation water for granulation. Granular acetylene carbon black is obtained after granulation. The granulated acetylene carbon black after granulation enters the drying device, and the drying temperature is 280°C. The granulated acetylene carbon black is sieved and tested, and the loss rate of acetylene carbon black is calculated.
[0075]
[0076] The loss rate of acetylene black = (the mass of the total feed - the granular acetylene black of the qualified particle size): the mass of the total feed * 100%
[0077] From the above table we can see that:
[0078] When the temperature of the wetting water is 80°C and the preheating temperature is raised to 40°C, the loss rate is 35°C. By gradually increasing the temperature, the loss rate decreases. When the preheating temperature reaches 80°C, the loss rate reaches the lowest value. When the preheating temperature continues to rise, the loss rate gradually increases.
[0079] When the temperature of the infiltration water is 50°C and the preheating temperature is raised to 60°C, it can be found that the average particle size is improved, which also means that the preheating method can not only reduce the loss rate but also reduce the temperature of the infiltration water.
[0080] When the temperature of the soaking water was 95°C and the preheating temperature was raised to 80°C, we found that the loss rate of acetylene black gradually increased.
[0081] What is disclosed above is only a preferred embodiment of the invention, which certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of implementing the above invention and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A method for granulating acetylene carbon black, Features: include a. Feed acetylene black and preheat the acetylene black at a temperature of 60°C; b. Adding wetting water to the acetylene black feed for wetting, the temperature of the wetting water is 50°C; c. granulating the impregnated acetylene carbon black to form granular acetylene carbon black, wherein the temperature of the granulation water is 75°C; d. Drying the granulated acetylene black to obtain an acetylene black product, wherein the drying temperature is 280°C.