A kind of corrosion-resistant adhesive tape and preparation method thereof

By using sheet-like graphene oxide and silane coupling agents to treat the tape, combined with suitable tackifiers and other additives, a cross-linked network structure is formed, which solves the problem of tape corrosion in humid environments and improves corrosion resistance and bonding strength.

CN115975536BActive Publication Date: 2024-11-08CHANGZHOU BAILU ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211668715.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-24
Publication Date
2024-11-08
Estimated Expiration
2042-12-24

AI Technical Summary

Technical Problem

Existing tapes are easily corroded by water, salt ions, and acid and alkali ions in humid environments, resulting in poor corrosion resistance and reduced adhesion.

Method used

Graphene oxide with a sheet structure is used as a preservative and treated with a silane coupling agent to form a cross-linked network structure. Combined with appropriate tackifier dosage and other additives such as fluoroether rubber and polystyrene nanospheres, the shielding effect and adhesion of the adhesive layer are improved.

Benefits of technology

It effectively prevents corrosive liquids from corroding the tape, maintains excellent adhesion, improves the tape's corrosion resistance and bonding strength, and reduces the risk of peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
  • Figure 796093DEST_PATH_IMAGE002
    Figure 796093DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The present application relates to the technical field of adhesive tape, and specifically discloses a corrosion-resistant adhesive tape and a preparation method thereof. A corrosion-resistant adhesive tape comprises a substrate and an adhesive layer, wherein the adhesive layer comprises the following weight parts of materials: 30-40 parts of thermoplastic rubber, 6-10 parts of tackifier, 1-2 parts of plasticizer, 1-2 parts of antioxidant, 1-2 parts of antioxidant, 1-3 parts of preservative, wherein the tackifier is selected from any one or more of petroleum resin C5, petroleum resin C9, terpene resin, and hydrogenated rosin resin, and the preservative comprises graphene oxide and graphene oxide treated with a silane coupling agent, and the graphene oxide is a lamellar structure. The adhesive tape composition of the present application can be used in the fields of electronic products, refrigerators, etc., and has the advantages of corrosion resistance, water resistance, and self-healing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adhesive tapes, and in particular to a corrosion-resistant adhesive tape and a preparation method thereof. Background Art

[0002] Aluminum foil tape is a tape formed by using aluminum foil as the base material and adhesive material on the aluminum foil. Aluminum foil tape usually has the advantages of excellent viscosity and strong adhesion. It is widely used in refrigerators, air conditioners, automobiles, pipelines, hotels, electronics and other industries. It can also be used in various electronic products such as PDA, PDP, LCD monitors, laptops, copiers, etc. where electromagnetic shielding is required.

[0003] With regard to the above-mentioned related technologies, most of the current tapes are easily corroded by water, salt ions, acid and alkali ions in water, etc. when used in pipelines or in humid environments. That is, the tapes have poor corrosion resistance, resulting in poor adhesion of the tapes. Summary of the invention

[0004] In order to improve the corrosion resistance and adhesion of the tape, the present application provides a corrosion-resistant tape and a preparation method thereof.

[0005] In a first aspect, the present application provides a corrosion-resistant tape, which adopts the following technical solution:

[0006] A corrosion-resistant tape comprises a substrate and an adhesive layer, wherein the adhesive layer comprises the following materials in parts by weight: 30-40 parts of thermoplastic rubber, 6-10 parts of tackifier, 1-2 parts of plasticizer, 1-2 parts of antioxidant, 1-2 parts of antioxidant, and 1-3 parts of preservative, wherein the tackifier is selected from any one or more of petroleum resin C5, petroleum resin C9, terpene resin, and hydrogenated rosin resin, and the preservative comprises graphene oxide and graphene oxide treated with a silane coupling agent, and the graphene oxide is a lamella structure.

[0007] By adopting the above technical solution, since the present application preferably uses graphene oxide with a lamellar structure as a preservative, the graphene oxide with a lamellar structure can be dispersed in the adhesive layer and connected to form a shielding layer, and the stacking between the layered structures is manifested as a staggered arrangement between the lamellar structures, so as to improve the shielding effect of the shielding layer and hinder the corrosion of the corrosive liquid to the tape. The surface and edge of the graphene oxide sheet with a lamellar structure contain more reactive sites, which not only improves the bonding effect between adjacent graphene oxides, but also improves the bonding firmness between graphene oxide and the remaining components in the adhesive layer, so it can play a role of layer-by-layer blocking.

[0008] Secondly, in the technical solution of the present application, graphene oxide treated with a silane coupling agent is preferably used as a preservative. The alcoholic hydroxyl groups in the silane coupling agent and the hydroxyl groups or carboxyl groups on the graphene oxide combine to form hydrogen bonds, which promote the combination between adjacent graphene sheets, forming a tightly bonded shielding layer, and effectively hindering the corrosion effect of the corrosive liquid on the adhesive layer. In addition, the dehydration between the silane molecules forms a stable Si-O-Si bond, gradually forming a cross-linked network structure, further improving the bonding firmness between the sheet graphene, and reducing the possibility of forming gaps between the shielding layers; and forming a double-layer structure of sheet graphene-cross-linked network structure. In addition, the dispersion effect of the sheet graphene modified by the silane coupling agent in the adhesive layer is further improved, so that a uniformly dispersed shielding layer can be formed in the sheet structure.

[0009] Finally, the amount of tackifier added is optimized in the technical solution of this application. The appropriate amount of tackifier added improves the wettability of the adhesive layer, allowing the adhesive layer to effectively wet the surface of the adherend and enhance the bonding effect of the tackifier. Even if the adhesive layer is corroded by corrosive liquid, the tape can still effectively maintain a better bonding effect and is not easy to peel off directly. If too much tackifier is added, the system will undergo a phase transition, the effect of the physical cross-linking points will be reduced, the intermolecular force will be weakened, and the adhesive force of the tape will decrease. Under the corrosion of the corrosive liquid, the tape is more susceptible to corrosion or debonding.

[0010] Preferably, the preservative further comprises fluoroether rubber or carboxyl nitrile rubber.

[0011] By adopting the above technical solution, the technical solution of this application preferably uses fluoroether rubber as a preservative, adds fluorine groups and fluorine structures in the adhesive layer, enhances the hydrophobic effect of the adhesive layer, and thus effectively blocks the corrosion of the adhesive layer by corrosive liquids, maintaining the excellent adhesive effect of the tape. The polar groups of carboxyl nitrile rubber are used to improve the compatibility between graphene oxide and the adhesive layer, and further improve the uniformity of the dispersion of the oxidative preservative in the adhesive layer, that is, the tape obtains a uniform corrosion resistance effect.

[0012] Preferably, the graphene oxide is graphene oxide modified by ionic liquid, and the ionic liquid is selected from 1-(2-aminoethyl)-3-methylimidazolium bromide or 1-methyl-3-propylaminoimidazole bis(trifluoromethylsulfonamide).

[0013] By adopting the above technical scheme, in the technical scheme of the present application, graphene oxide is preferably modified with ionic liquid, and the ionic liquid can react with the carboxyl, hydroxyl, epoxy and carbonyl groups on the graphene oxide, or obtain graphene oxide with a loose and porous morphology, and the fluorine-containing structure in the ionic liquid and the fluoroether rubber can form interchain interactions to form physical cross-linking points, which not only further improves the adhesive strength of the adhesive layer, but also improves the dispersion uniformity and compatibility of graphene oxide in the adhesive layer, and can form a uniform shielding layer structure in the adhesive layer to improve the corrosion resistance of the tape.

[0014] At the same time, the ionic liquid can also react with the silane groups on the graphene oxide treated with the silane coupling agent to form a hybrid nanomaterial to improve the density of the shielding layer and reduce the pore structure on the shielding layer.

[0015] Preferably, polystyrene nanospheres are loaded on the graphene oxide.

[0016] By adopting the above technical scheme, in the technical scheme of the present application, polystyrene nano-microspheres are loaded on the graphene oxide with a lamellar structure. The microsphere structure of polystyrene can effectively prevent the stacking of the graphene oxide lamellar structure, improve the dispersion uniformity of graphene oxide in the adhesive material to form a uniform shielding layer, and the polyethylene microspheres can also fill the gaps between the graphene oxide, thereby improving the density of the shielding layer and reducing the corrosion of the adhesive layer by the corrosive liquid.

[0017] In addition, graphene oxide and polystyrene nanospheres promote each other's dispersion, forming a complete filler network and a stronger interfacial bonding effect in the adhesive layer, increasing the physical and chemical cross-linking points, so that the density of the shielding layer is further improved, and the viscosity of the adhesive layer is also improved. Therefore, it can not only effectively block the corrosive liquid, but also maintain excellent adhesion.

[0018] Preferably, the preparation method of the polystyrene nanospheres comprises the following steps: stirring and mixing cetyltrimethylammonium bromide (CTAB), styrene and divinylbenzene, ultrasonic pre-emulsification, constant temperature reaction, adding initiator, continuously stirring the reaction, cooling, discharging, and obtaining a polystyrene microsphere solution.

[0019] By adopting the above technical scheme, the preparation steps of polystyrene microspheres are optimized in the technical scheme of the present application, and the appropriate preparation method makes the spherical structure of the polystyrene nanospheres complete and the particle size uniform, so that the nanospheres can effectively separate the graphene oxide and fill the pores between the lamellar structures, thereby improving the anti-corrosion effect of the tape.

[0020] Preferably, the preservative further comprises sinacamidopropyl betaine viscoelastic, and the sinacamidopropyl betaine viscoelastic is sinacamidopropyl betaine viscoelastic modified by a silane coupling agent.

[0021] By adopting the above technical solution, the technical solution of this application preferably adopts the addition of sinacamidopropyl betaine viscoelastic in the adhesive layer. The sinacamidopropyl betaine viscoelastic has a long hydrophobic carbon chain and is surface active, which not only improves the viscoelasticity of the adhesive layer, but also improves the hydrophobic effect of the adhesive layer, effectively blocking corrosive liquids. Moreover, after the adhesive layer contacts with acid, the acid and the sinacamidopropyl betaine viscoelastic form stable micelles, further improving the adhesiveness and peeling resistance of the adhesive layer.

[0022] Secondly, the mustard amide propyl betaine viscoelastic is modified by a silane coupling agent, and the dispersion effect of the mustard amide propyl betaine viscoelastic in the adhesive layer is improved through a grafting reaction, so that the adhesive layer obtains a uniform hydrophobic and viscoelastic effect.

[0023] Preferably, the preservative comprises hydrophobic microspheres, the hydrophobic microspheres are sulfonate betaine gel microspheres, and the sulfonate betaine gel is hydrophobically modified by a hydrophobic monomer.

[0024] By adopting the above technical scheme, sulfonated betaine gel microspheres are added to the adhesive layer in this application, and the surface of the hydrophobic microspheres is a hydrophilic layer-sulfonated betaine gel structure. When the adhesive layer meets water, the hydrophilic layer of the hydrophobic microspheres absorbs water and breaks to release the sulfonated betaine gel structure. The sulfonated betaine gel structure has an excellent self-healing effect by itself, so the sulfonated betaine gels in adjacent hydrophobic microspheres can combine with each other to form a cross-linked network structure, further enhancing the density of the adhesive layer and hindering the possibility of the corrosive liquid continuing to corrode the tape. And after part of the gel structure is corroded, with the end of the corrosion, the sulfonated betaine gel structure will self-heal again, restore the complete cross-linked network structure, improve the density of the adhesive layer, and improve the corrosion resistance of the tape.

[0025] In the present application, it is preferred to use a hydrophobic monomer to hydrophobically modify the sulfonated betaine gel. The addition of the hydrophobic monomer can release the hydrophobic sulfonated betaine gel after the outer layer of the hydrophobic microspheres is broken, forming a cross-linked network structure with a hydrophobic function, further hindering the possibility of corrosive liquids or water eroding the adhesive material. In addition, due to the coordination between the hydrophobic interaction and the ionic bond, the self-healing effect of the sulfonated betaine gel is improved, that is, it promotes the formation of a dense cross-linked network in the adhesive layer, and improves the corrosion resistance and hydrophobic effect of the adhesive layer.

[0026] Preferably, a co-solvent is added during the hydrophobic modification treatment, and the co-solvent is selected from sodium dodecyl sulfate or hexadecyltrimethylammonium chloride.

[0027] By adopting the above technical scheme, sodium dodecyl sulfate is used as a cosolvent, and there are multiple crosslinks between the cosolvent and the hydrophobic microspheres. When the sulfonated betaine gel network is broken, the hydrophobic segments and ionic bonds can jump to maintain the gel crosslinked network. In addition, the molecular chains in the sulfonated betaine gel are brought closer to each other in a curved manner, further improving the toughness of the crosslinked network, so that the crosslinked network can withstand the impact of a certain amount of water and corrosive liquids. After the sulfonated betaine gel network is broken, the hydrophobic groups are wrapped in the gel, and the sodium dodecyl sulfate and the side chain anions and cations quickly return to the original position to repair the hydrophobic and ionic bonds, thereby realizing a self-healing crosslinked network and maintaining the dense effect in the adhesive layer.

[0028] Hexadecyltrimethylammonium chloride is used as a cosolvent, which is easier to attract ions with the other components in the hydrophobic microspheres. After the sulfonate betaine gel network is broken, the positive and negative ions at the break quickly form bonds to achieve self-healing and maintain the integrity of the gel network.

[0029] Preferably, the substrate is selected from any one of aluminum foil, PET, tissue paper, and PVC.

[0030] In a second aspect, the present application provides a method for preparing a corrosion-resistant tape, using the following technical solution:

[0031] A method for preparing a corrosion-resistant adhesive tape comprises the following steps: mixing thermoplastic rubber, a tackifier, a plasticizer, an anti-aging agent, an antioxidant and a preservative by stirring, melting and mixing, brushing on a substrate and drying to obtain the corrosion-resistant adhesive tape.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. Since the present application uses graphene oxide with a lamellar structure as a preservative, the graphene oxide with a lamellar structure can be dispersed and form a shielding layer, and the staggered arrangement between the lamellar structures improves the shielding effect of the shielding layer and hinders the corrosion of the corrosive liquid to the tape. The surface and edge of the graphene oxide sheet with a lamellar structure contain more reactive sites, which not only improves the bonding effect between adjacent graphene oxides, but also improves the bonding firmness between graphene oxide and the other components in the adhesive layer, so it can play a role of layer-by-layer blocking.

[0034] Secondly, the silane coupling agent modifies the graphene oxide to form hydrogen bonds, promote the bonding between adjacent graphene sheets, and form a tightly bonded shielding layer. In addition, the silane molecules are dehydrated to form stable Si-O-Si bonds, gradually forming a cross-linked network structure, further improving the bonding firmness between the graphene sheets; forming a double-layer structure of graphene sheets-cross-linked network structure. In addition, the dispersibility of the graphene sheets modified by the silane coupling agent in the adhesive layer is further improved, so that a uniformly dispersed shielding layer can be formed in the sheet structure.

[0035] Finally, the amount of tackifier added is optimized in the technical solution of the present application. The appropriate amount of tackifier added improves the wettability of the adhesive layer, allowing the adhesive layer to effectively wet the surface of the adherend and enhance the bonding effect of the tackifier. Even if the adhesive layer is corroded by corrosive liquid, the tape can still effectively maintain a better bonding effect and is not easy to be directly peeled off.

[0036] 2. In the present application, it is preferred to load polystyrene nanospheres on graphene oxide. The polystyrene microsphere structure prevents the stacking of graphene oxide sheet structures, improves the dispersion uniformity of graphene oxide in the adhesive material, and can also fill the gaps between graphene oxides, thereby improving the compactness of the shielding layer and reducing the corrosion of the adhesive layer by the corrosive liquid.

[0037] In addition, graphene oxide and polystyrene nanospheres promote each other's dispersion, forming a complete filler network and a stronger interface bonding effect in the adhesive layer, increasing the physical and chemical cross-linking points, so that the density of the shielding layer is further improved, and the viscosity of the adhesive layer is further improved.

[0038] 3. In the present application, it is preferred to add a mustard amide propyl betaine viscoelastic body to the adhesive layer. The mustard amide propyl betaine viscoelastic body has a long hydrophobic carbon chain and is surface active, which not only improves the viscoelasticity of the adhesive layer, but also improves the hydrophobic effect of the adhesive layer, effectively blocking the corrosive liquid. Moreover, after the adhesive layer contacts with the acid, the acid and the mustard amide propyl betaine viscoelastic body form stable micelles, further improving the adhesiveness and peeling effect of the adhesive layer.

[0039] Secondly, the mustard amide propyl betaine viscoelastic is modified by a silane coupling agent, and the dispersion effect of the mustard amide propyl betaine viscoelastic in the adhesive layer is improved through a grafting reaction, so that the adhesive layer obtains a uniform hydrophobic and viscoelastic effect. DETAILED DESCRIPTION

[0040] The present application is further described in detail below with reference to the embodiments.

[0041] In the embodiments of the present application, the instruments and equipment used are as follows, but not limited thereto:

[0042] Preparation Example

[0043] Thickener Preparation Example

[0044] Preparation Example 1

[0045] Take 10 kg of petroleum resin C5 as a tackifier. The tackifier includes but is not limited to: any one or more of petroleum resin C5, petroleum resin C9, terpene resin, and hydrogenated rosin resin.

[0046] Preservative Preparation Example

[0047] Preparation Example 2

[0048] The graphene oxide was immersed in a silane coupling agent (1,2-bis(triethoxysilyl)ethane) solution, filtered, and washed to obtain graphene oxide treated with a silane coupling agent. 3 kg of flaky graphene oxide was mixed with 3 kg of graphene oxide treated with a silane coupling agent as preservative 1.

[0049] Preparation Example 3

[0050] 3 kg of flaky graphene oxide, 3 kg of graphene oxide treated with a silane coupling agent, and 1 kg of fluoroether rubber were mixed to serve as preservative 2.

[0051] Preparation Example 4

[0052] 3 kg of flaky graphene oxide, 3 kg of graphene oxide treated with a silane coupling agent, and 1 kg of carboxylated nitrile rubber were mixed as preservative 3.

[0053] Preparation Example 5

[0054] The graphene oxide is immersed in a 1-(2-aminoethyl)-3-methylimidazolium bromide solution and filtered to obtain the graphene oxide modified by the ionic liquid. 3 kg of the graphene oxide modified by the ionic liquid, 3 kg of the graphene oxide treated by the silane coupling agent, and 1 kg of fluoroether rubber are mixed to serve as the preservative 4.

[0055] The ionic liquid includes, but is not limited to, 1-(2-aminoethyl)-3-methylimidazolium bromide or 1-methyl-3-propylaminoimidazole bis(trifluoromethylsulfonamide).

[0056] Preparation Example 6

[0057] 3 kg of flaky graphene oxide, 2 kg of graphene oxide modified by ionic liquid, 3 kg of graphene oxide treated by silane coupling agent, and 1 kg of fluoroether rubber were mixed to serve as preservative 5.

[0058] Preparation Example 7

[0059] The difference from Preparation Example 2 is that 6 g of hexadecyltrimethylammonium bromide (CTAB), 90 g of styrene, 10 g of divinylbenzene and 1 L of water are stirred and mixed at 150 r / min, ultrasonically pre-emulsified at 50° C. for 30 min, reacted at a constant temperature of 70° C., 1 g of initiator KPS is added, the reaction is continued with stirring for 5 h, cooled to 40° C., and discharged to obtain a polystyrene microsphere solution.

[0060] The graphene oxide was dispersed in water to obtain a 1 g / L dispersion, the dispersion was added to a polystyrene microsphere solution, hydrazine hydrate was added, heated under reflux at 90° C. for 10 h, and the hybrid filler powder was obtained by centrifugation, water washing, and vacuum drying.

[0061] Hybrid filler powder was used to replace the graphene oxide in Preparation Example 2 to prepare graphene oxide treated with a silane coupling agent, and then to prepare preservative 6.

[0062] Preparation Example 8

[0063] The difference from Preparation Example 7 is that the hybrid filler powder and the graphene oxide treated with a silane coupling agent in Preparation Example 2 are used to prepare the preservative 7.

[0064] Preparation Example 9

[0065] The difference from Preparation Example 2 is that 3 kg of flaky graphene oxide, 1 kg of mustard amide propyl betaine viscoelastic, and 3 kg of graphene oxide treated with a silane coupling agent are mixed to prepare preservative 8.

[0066] The preparation of the sinacamidopropyl betaine viscoelastic body comprises the following steps: taking 2 kg of sinacamidopropyl betaine and 0.1 kg of silane coupling agent KH550, stirring and mixing, and obtaining a sinacamidopropyl betaine viscoelastic body modified by the silane coupling agent.

[0067] Preparation Example 10

[0068] The difference from Preparation Example 2 is that: 1 mol DMAPS (3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt), 0.3 mol polyethylene glycol acrylate, 1 mol initiator APS, 1 mol 2,2,2-trifluoroethyl methyl methacrylate (FMA), 0.5 mol sodium dodecyl sulfate and 1 L water are ultrasonically oscillated and free radical polymerization is initiated in a water bath at 60°C nitrogen atmosphere to obtain sulfonated betaine gel. The sulfonated betaine gel is crushed to obtain sulfonated betaine gel particles, gelatin is sprayed on the sulfonated betaine gel particles, and dried and solidified to obtain hydrophobic microspheres.

[0069] 3 kg of flaky graphene oxide, 1 kg of hydrophobic microspheres, and 3 kg of graphene oxide treated with a silane coupling agent were mixed to prepare a preservative 9.

[0070] Preparation Example 11

[0071] 3 kg of flaky graphene oxide, 1 kg of hydrophobic microspheres, 1 kg of mustard amide propyl betaine viscoelastic, and 3 kg of graphene oxide treated with a silane coupling agent were mixed to prepare a preservative 10.

[0072] Preparation Example 12

[0073] The difference from Preparation Example 10 is that hexadecyltrimethylammonium chloride is used to replace the sodium dodecyl sulfate in Preparation Example 10 to prepare preservative 11. Example

[0074] Examples 1-3

[0075] On the one hand, the present application provides a corrosion-resistant tape, including a substrate and an adhesive layer, wherein the adhesive layer is loaded on the substrate, and the adhesive layer comprises thermoplastic rubber, tackifier, plasticizer, antioxidant, antioxidant, and preservative 1, and the specific mass is shown in Table 1. The thermoplastic rubber is SIS thermoplastic elastomer, and the tackifier is petroleum resin C5.

[0076] The substrate includes, but is not limited to, any one of aluminum foil, PET, tissue paper, and PVC. In this embodiment, aluminum foil is selected as the substrate.

[0077] On the other hand, the present application provides a method for preparing a corrosion-resistant tape, comprising the following steps: stirring and mixing thermoplastic rubber, tackifier, plasticizer, antioxidant, antioxidant, and preservative 1, melt mixing, coating with film by a coater, rolling semi-finished products, cutting tubes, slitting with a slitting machine, packaging, and encapsulating to obtain finished corrosion-resistant tapes 1-3.

[0078] Table 1 Composition of adhesive layer of Examples 1-3

[0079] Embodiment 4-13

[0080] The difference from Example 1 is that preservative 2-11 is used to replace preservative 1 in Example 1 to prepare corrosion-resistant tapes 4-13.

[0081] Comparative Example

[0082] Comparative Example 1

[0083] The difference between this comparative example and Example 1 is that in this comparative example, 10 kg of terpene resin is preferably used as a tackifier to prepare the corrosion-resistant tape 14.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 3 is that in this comparative example, only graphene oxide is added as a preservative to prepare the corrosion-resistant tape 15.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 3 is that in this comparative example, only graphene is added as a preservative to prepare the corrosion-resistant tape 16.

[0088] Comparative Example 4

[0089] The difference between this comparative example and Example 3 is that no preservative is added in this comparative example to prepare the corrosion-resistant tape 17.

[0090] Performance testing

[0091] (1) Peel strength: The peel strength of the corrosion-resistant tape is tested according to GBT 2792-2014 Test method for peel strength of adhesive tape.

[0092] (2) Corrosion resistance test: Test the waterproof effect of the corrosion-resistant tape according to GB / T 18173.1-2006 Physical performance test of pressure-sensitive rubber waterproof membrane;

[0093] (3) Adhesion performance test: The adhesion of the corrosion-resistant tape is tested according to the national standard "GB / T 4851-2014 Test method for adhesion of adhesive tapes".

[0094] Table 2 Performance test of Examples 1-13 and Comparative Examples 1-4

[0095]

[0096] In the embodiments of the present application, the tensile strength is ≥3 kN / m, the bonding rate with polyurethane is ≥60%, the adhesion at room temperature is ≥170 min, the adhesion at high temperature is ≥15 min, and the high temperature peel strength is ≥0.5 kN / m.

[0097] Combining the performance test comparison in Table 2, we can find that:

[0098] (1) By comparing Examples 1-3 with Comparative Examples 1-4, it can be found that the corrosion resistance, peel strength and stickiness of the corrosion-resistant tapes prepared in Examples 1-3 are all improved, which indicates that the amount of tackifier added is optimized in the present application. The appropriate amount of tackifier added improves the wettability of the adhesive layer, enhances the bonding effect of the tackifier, and is not easy to peel directly. By comparing Example 3 with Comparative Example 1, it can be found that when too much tackifier is added, the system undergoes a phase transition, the effect of the physical crosslinking points is reduced, the intermolecular force is weakened, and the stickiness of the tape is reduced. Under the corrosion of the corrosive liquid, the tape is more easily corroded or debonded.

[0099] The lamellar graphene oxide acts as a preservative. The lamellar graphene oxide can be dispersed in the adhesive layer and connected to form a shielding layer. The stacking between the layered structures is manifested as an interlaced arrangement between the lamellar structures, so as to improve the shielding effect of the shielding layer and prevent the corrosion of the tape by the corrosive liquid.

[0100] (2) By comparing Examples 4-5 with Example 1, it can be found that the corrosion resistance, peel strength and adhesion retention of the corrosion-resistant tape prepared in Examples 4-5 are all improved. The present application uses fluoroether rubber or carboxyl nitrile rubber as a preservative, and adds fluorine groups and fluorine structures to the adhesive layer to enhance the hydrophobic effect of the adhesive layer, thereby effectively blocking the erosion of the adhesive layer by the corrosive liquid and maintaining the excellent adhesive effect of the tape.

[0101] (3) By comparing Examples 6-7 with Example 1, it can be found that the corrosion resistance, peel strength and adhesion of the corrosion-resistant tape prepared in Examples 6-7 are all improved. In the present application, graphene oxide is modified by ionic liquid, and graphene oxide can obtain a relatively loose and porous morphology. In addition, the fluorine-containing structure in the ionic liquid and the fluoroether rubber can form interchain interactions to form physical cross-linking points, which not only further improves the adhesive strength of the adhesive layer, but also improves the dispersion uniformity and compatibility of graphene oxide in the adhesive layer, and can form a uniform shielding layer structure in the adhesive layer to improve the corrosion resistance of the tape.

[0102] (4) By comparing Examples 8-9 with Example 1, it can be found that the corrosion resistance, peel strength and adhesion of the corrosion-resistant tape prepared in Examples 8-9 are all improved. The present application uses graphene oxide and polystyrene nanospheres to promote the dispersion of each other, forming a complete filler network and a stronger interface adhesion effect in the adhesive layer, increasing the physical and chemical cross-linking points, so that the density of the shielding layer is further improved, and the viscosity of the adhesive layer is further improved. Therefore, it can not only effectively block the corrosive liquid, but also maintain excellent adhesion.

[0103] (5) By comparing Example 10, Examples 11-13 and Example 1, it can be found that the corrosion resistance, peel strength and adhesion of the corrosion-resistant tapes prepared in Examples 10-13 are all improved. The addition of viscoelastics to the preservatives in this application not only improves the viscoelasticity of the adhesive layer, but also improves the hydrophobic effect of the adhesive layer, effectively blocking the corrosive liquid. After the adhesive layer contacts the acid, the acid and the sinacamidopropyl betaine viscoelastic form stable micelles, further improving the adhesion and peeling effect of the adhesive layer.

[0104] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A corrosion-resistant tape, characterized in that: The invention comprises a substrate and an adhesive layer, wherein the adhesive layer comprises the following materials in parts by weight: 30-40 parts of thermoplastic rubber, 6-10 parts of tackifier, 1-2 parts of plasticizer, 1-2 parts of antioxidant, 1-2 parts of antioxidant, and 1-3 parts of preservative, wherein the tackifier is selected from any one or more of petroleum resin C5, petroleum resin C9, terpene resin, and hydrogenated rosin resin, and the preservative comprises graphene oxide and graphene oxide treated with a silane coupling agent, wherein the graphene oxide is a sheet structure, and polystyrene nanospheres are loaded on the graphene oxide.

2. A corrosion-resistant tape according to claim 1, characterized in that: The preservative also includes fluoroether rubber or carboxyl nitrile rubber.

3. A corrosion-resistant tape according to claim 2, characterized in that: The graphene oxide is graphene oxide modified by ionic liquid, and the ionic liquid is selected from 1-(2-aminoethyl)-3-methylimidazolium bromide or 1-methyl-3-propylaminoimidazole bis(trifluoromethylsulfonamide).

4. The corrosion-resistant tape according to claim 1, characterized in that: The preparation method of polystyrene nanospheres comprises the following steps: mixing cetyltrimethylammonium bromide (CTAB), styrene and divinylbenzene, ultrasonic pre-emulsification, constant temperature reaction, adding initiator, continuously stirring reaction, cooling, discharging, and obtaining a polystyrene microsphere solution.

5. The corrosion-resistant tape according to claim 1, characterized in that: The preservative further comprises sinacamidopropyl betaine viscoelastic body, and the sinacamidopropyl betaine viscoelastic body is sinacamidopropyl betaine viscoelastic body modified by silane coupling agent.

6. The corrosion-resistant tape according to claim 1, characterized in that: The preservative comprises hydrophobic microspheres, which are sulfonate betaine gel microspheres, and the sulfonate betaine gel is hydrophobically modified by a hydrophobic monomer.

7. The corrosion-resistant tape according to claim 6, characterized in that: A cosolvent is added during the hydrophobic modification treatment, and the cosolvent is selected from sodium dodecyl sulfate or hexadecyltrimethylammonium chloride.

8. The corrosion-resistant tape according to claim 1, characterized in that: The substrate is selected from any one of aluminum foil, PET, tissue paper, and PVC.

9. A method for preparing a corrosion-resistant tape according to any one of claims 1 to 7, characterized in that: The following steps are involved: Thermoplastic rubber, tackifier, plasticizer, antioxidant, antioxidant and preservative are stirred and mixed, melted and mixed, brushed on a substrate, and cooled to obtain a corrosion-resistant tape.