A UV moisture dual curing polyurethane hot melt adhesive
By synthesizing modified polyurethane acrylic resin containing double bonds and difunctional isocyanate groups in polyurethane hot melt adhesive, combined with efficient photoinitiator and self-made cross-linking agent, the problems of slow moisture reaction and insufficient UV light are solved and achieved The rapid curing and high bonding strength of UV moisture dual-curing polyurethane hot melt adhesive improves production efficiency and bonding stability.
Patent Information
- Application Number
- CN202211607425.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Existing reactive polyurethane hot melt adhesives react slowly to moisture and require pressure holding and special molds, which affects production efficiency. In addition, the glue parts that are not fully exposed to UV light lead to a decrease in bonding strength and aging performance.
UV moisture dual-curing polyurethane hot melt adhesive is used to achieve rapid curing and high bonding strength by synthesizing modified polyurethane acrylic resin containing double bonds and difunctional isocyanate groups, combined with efficient photoinitiators and self-made cross-linking agents. And it still maintains good performance under insufficient UV light conditions.
It achieves a pressure-free process, has good initial bonding strength and mechanical properties, and maintains high bonding strength and aging performance under insufficient light conditions, improving production efficiency and bonding stability.
Smart Images

Figure BDA0003998350910000071
Abstract
Description
Technical Field
[0001] The invention relates to a UV-moisture dual-curing polyurethane hot melt adhesive, belonging to the technical field of adhesives. Background Art
[0002] Reactive polyurethane hot melt adhesive is an environmentally friendly hot melt adhesive. It not only has the easy-to-operate process characteristics of ordinary hot melt adhesive, but also contains active isocyanate groups. It can still undergo curing and cross-linking reactions with moisture in the air at room temperature, thereby obtaining excellent bonding properties, good flexibility and weather resistance, etc. Therefore, it is widely used in consumer electronics, woodworking, home appliances, textiles and other industries.
[0003] Because moisture reaction is slow and takes time to reach a certain strength, practical applications usually require pressure holding, which requires special molds and a certain pressure holding time, increasing costs and affecting production efficiency. Therefore, UV moisture dual-curing reactive polyurethane hot melt adhesives have begun to be widely studied in order to achieve rapid positioning, improve production efficiency, and at the same time, the cured product has good mechanical properties and aging resistance of reactive polyurethane hot melt adhesives.
[0004] Due to the irregularity of the actual bonding samples, the glue parts that were not fully exposed to UV light did not react, resulting in a decrease in bonding strength and aging performance, leading to bonding failure. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a UV moisture dual-curing polyurethane hot melt adhesive and a preparation method thereof. The prepared UV moisture curable polyurethane hot melt adhesive not only has good initial bonding strength and can realize a pressure-free process, but also has good mechanical properties after being fully cured, and still has good bonding strength even under insufficient UV light conditions.
[0006] The technical solution of the present invention for solving the above technical problems is as follows: it comprises, by weight: 30 to 80 parts of polyol polymer C, 10 to 40 parts of isocyanate compound, 0.1 to 70 parts of self-made modified polyurethane acrylate, 0.01 to 3 parts of catalyst, 0.01 to 10 parts of self-made cross-linking agent, 0.1-5 parts of photoinitiator, and 2-20 parts of tackifying resin.
[0007] Further, the synthesis steps of the homemade modified polyurethane acrylate are as follows:
[0008] 20-80 parts of polyol A and 10-50 parts of polyol B after dehydration treatment are heated to 65-100°C, 20-60 parts of isocyanate compound are added, the temperature is raised to 100-120°C, the reaction is carried out under vacuum for 30-120 minutes, the temperature is then lowered to 85°C, 0.001-0.1 parts of polymerization inhibitor are added, and the mixture is fully stirred, 10-80 parts of low molecular weight hydroxy acrylate are added, the temperature is raised to 85-120°C, the reaction is carried out under vacuum for a period of time, 0.01-1 parts of catalyst are added, the reaction is carried out under vacuum for 30-120 minutes, 0.001-0.1 parts of water removing agent are added after the reaction is complete, and the mixture is sealed and stored to obtain a self-made modified polyurethane acrylic resin.
[0009] The polyol A is a polyol with a functionality of 3 and a molecular weight between 400 and 10,000; it includes one or a mixture of polyether triol, polycaprolactone triol and castor oil triol.
[0010] The polyol B is a polyester or polyether polyol with a functionality of 4, such as polycaprolactone tetraol, polyether tetraol polyol pep 550, etc.
[0011] Further, the synthesis steps of the homemade cross-linking agent are as follows:
[0012] Heat 0.1-80 parts of the multifunctional isocyanate siloxane after dehydration treatment to 85°C, add 0.001-0.01 parts of inhibitor and stir well, add 20-50 parts of low molecular weight hydroxy acrylate, add 0.01-1 parts of catalyst and heat to 100-120°C, react for 60-240 minutes under vacuum, add 0.001-0.1 parts of dehydrating agent after the reaction is complete, seal and store to obtain a homemade cross-linking agent.
[0013] The polyfunctional isocyanate siloxane is a long-chain siloxane compound containing a plurality of isocyanate groups and a plurality of alkoxy functional groups, and Shin-Etsu X-12-1159L is an example.
[0014] The isocyanate compound is a polyisocyanate compound, including one or a mixture of methylene diphenyl diisocyanate (MDI), liquefied methylene diphenyl diisocyanate (MDI), hydrogenated methylene diphenyl diisocyanate (HMDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), polymerized methylene diphenyl diisocyanate, toluene diisocyanate (TDI), polymethylene polyphenyl diisocyanate, naphthalene diisocyanate (NDI) or polymethylene polyphenyl isocyanate (PAPI).
[0015] The low molecular weight hydroxy acrylate is a low molecular weight methacrylic resin or acrylic resin containing a hydroxyl group with a molecular weight greater than 300 and a boiling point greater than 200° C. It includes but is not limited to methacrylate or caprolactone acrylate.
[0016] The inhibitor is an inhibitor commonly used for free radical compounds, including phenol, MEHQ (p-hydroxyanisole), PTZ (phenothiazine), THQ (methylhydroquinone), tris (N-nitroso-N-phenylhydroxylamine) aluminum salt or a combination of more than one of them.
[0017] The dewatering agent includes oxazolidines, monofunctional isocyanates, and monofunctional siloxanes.
[0018] The polyol polymer C is a polyester polyol polymer with a molecular weight of 300-8000, a polyether polyol polymer, or a mixture of one or more of polymers containing hydroxyl functional groups; the polyester polyol polymer includes a common polyester polyol polymer, a polycaprolactone polyol polymer, and a polycarbonate polyol polymer; the common polyester polyol is a polymer produced by reacting an acid or an acid anhydride with a corresponding alcohol, and is produced by reacting at least one of adipic acid, sebacic acid, dodecanoic acid, isophthalic acid, terephthalic acid, phthalic acid, and phthalic anhydride with 1,4-butanediol, diethylene glycol, neopentyl glycol, ethylene glycol, cyclohexanediol, diol The polyol is obtained by polymerizing at least one of glycol, 1,6-hexanediol and 3-methyl-1,5-pentanediol; the polycaprolactone polyol is a poly-ε-caprolactone polyol obtained by ring-opening polymerization of ε-caprolactone; the polycarbonate polyol is a polymer containing a polycarbonate group, such as polycarbonate 1,6-hexanediol ester polyol, pentanediol, hexanediol, butanediol, propylene glycol and other copolymer polyesters, polycyclohexane carbonate glycol ester polyol or several thereof; the polyether polyol includes ring-opening polymers of ethylene glycol, propylene glycol, tetrahydrofuran, 3-methyltetrahydrofuran, and random copolymers or block copolymers of them or their derivatives. Examples include Evonik's 7360, 7255, etc.
[0019] The tackifying resin is one or a mixture of terpene resin, rosin resin and petroleum resin.
[0020] The catalyst is one or more of dibutyltin dilaurate, stannous octoate, dibutylene acetate, triethylenediamine, and bismorpholinyl diethyl ether (DMDEE).
[0021] The photoinitiator is a commonly used initiator for free radical polymerization, and may be one of 189, 1173, TPO, TPO-L, 907, 184 or a combination of more than one thereof.
[0022] The beneficial effects of the present invention are as follows: by selecting suitable raw materials and optimizing the modification process, a modified polyurethane acrylic resin containing partial double bonds and NCO content is synthesized. The modified acrylic resin contains double bonds that can undergo UV curing reactions and difunctional isocyanate groups. After UV irradiation, it can provide good immediate initial strength and react into the PUR bulk resin during the moisture reaction process of post-curing to provide good strength. In the absence of sufficient light, the late wet curing can still undergo a chain extension reaction with the PUR part to obtain good bonding and aging properties. At the same time, a self-made cross-linking agent with higher double bond density and NCO density is added, and a small amount of the modified polyurethane acrylic resin is added to improve the initial strength after UV irradiation and the final curing strength without UV irradiation. The introduced multifunctional siloxane can improve the final bonding force of the glue to the substrate, and at the same time, it helps the system to bond at the interface during the aging process, and can play the role of a coupling agent even without light. DETAILED DESCRIPTION
[0023] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0024] (1) Synthesis of homemade modified acrylic polyurethane:
[0025] Heat the mixture of 67 parts of dehydrated Bluestar Dongda EP-3600 and 2 parts of polyol pep 550 to 80°C, add 12.9 parts of MDI, heat to 100°C, react at a stirring speed of 400r / min under vacuum conditions for 1h, cool to 60-80°C, add 0.05 parts of MEHQ, stir well, add 18 parts of caprolactone acrylate, heat to 85-100°C, vacuum react for 2-5 hours, test to reach the theoretical NCO content, add 0.05 parts of oxazolidine, discharge, and seal for storage.
[0026] (2) Synthesis of homemade cross-linking agent:
[0027] Heat 50.3 parts of multifunctional isocyanate siloxane after dehydration treatment to 85°C, add 0.05 parts of phenol and stir well, add 49.6 parts of caprolactone acrylate and heat to 85-120°C, react under vacuum for 60-240 minutes, add 0.05 parts of oxazolidine after the reaction is complete, seal and store to obtain a homemade cross-linking agent.
[0028] (3) Synthesis of polyurethane hot melt adhesive:
[0029] Step 1: 30-80 parts of polyol polymer C and 2-20 parts of tackifying resin are heated to 120-140°C and vacuum dehydrated for 2 hours at 300 r / min stirring;
[0030] Step 2: Cool down to 100°C, continue to add 10 to 40 parts of polyisocyanate compounds, raise the temperature to 110°C, react at a stirring speed of 450r / min under vacuum conditions for 1h, add 0.1 to 70 parts of homemade modified polyurethane acrylate, 0.01 to 10 parts of homemade cross-linking agent, 0.01 to 3 parts of catalyst, 0.1 to 5 parts of photoinitiator, stir under vacuum conditions for 30min, then discharge the material, vacuum seal and store away from light.
[0031] Example 1
[0032] 24 parts of poly(hexylene adipate) diol with a molecular weight of 3500, 19 parts of poly(neopentyl adipate) diol with a molecular weight of 2000, 16 parts of polytetramethylene glycol ether diol with a molecular weight of 2000, and 5 parts of petroleum resin were added to a reaction bottle by weight, heated to 120-140°C, and vacuum dehydrated for 2 hours at a stirring condition of 300 / min; then, the temperature was lowered to 100°C, 13.9 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, the temperature was raised to 110°C, and the reaction was carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 20 parts of modified polyurethane acrylate, 1 part of a homemade crosslinking agent, 0.1 part of DMDEE, and 1 part of TPO were added, and the mixture was stirred at a stirring speed of 450r / min under vacuum conditions for 30 minutes before discharging the mixture and vacuum sealing and light protection were stored.
[0033] Example 2
[0034] 21 parts of poly(hexylene adipate) diol with a molecular weight of 3500, 19 parts of poly(neopentyl adipate) diol with a molecular weight of 2000, 20 parts of poly(oxypropylene) diol with a molecular weight of 2000, and 3.8 parts of petroleum resin were added to a reaction bottle by weight, heated to 120-140°C, and vacuum dehydrated for 2 hours at a stirring condition of 300 / min; then, the temperature was lowered to 100°C, 13.9 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, the temperature was raised to 110°C, and the reaction was carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 19 parts of modified polyurethane acrylate, 1.5 parts of a homemade crosslinking agent, 0.12 parts of DMDEE, and 1.5 parts of 819 were added, and the mixture was stirred at a stirring speed of 450r / min under vacuum conditions for 30 minutes before being discharged and vacuum-sealed and stored away from light.
[0035] Example 3
[0036] 18 parts of poly(hexane adipate glycol) diol with a molecular weight of 3500, 20 parts of poly(caprolactone diol) with a molecular weight of 2000, 12 parts of polycarbonate diol with a molecular weight of 1000, and 2 parts of petroleum resin were added to a reaction bottle by weight, heated to 120-140°C, and vacuum dehydrated for 2 hours at 350 r / min stirring conditions; then, the temperature was lowered to 100°C, 14.9 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, and the reaction was carried out at a stirring speed of 450 r / min under vacuum conditions for 1 hour, and then 30 parts of modified polyurethane acrylate, 2 parts of homemade crosslinking agent, 0.1 part of DMDEE, and 1 part of 907 were added. The mixture was stirred at a stirring speed of 450 r / min under vacuum conditions for 30 minutes, then discharged, and vacuum-sealed and stored away from light.
[0037] Example 4
[0038] 20 parts of polybutylene adipate polyol with a molecular weight of 2000, 20 parts of polyoxypropylene glycol with a molecular weight of 1000, 12 parts of polyhexamethylene phthalate diol with a molecular weight of 1000, and 8 parts of petroleum resin are added to a reaction bottle by weight, heated to 130-140°C, and vacuum dehydrated for 2 hours at 350 r / min stirring conditions; then, the temperature is lowered to 100°C, 20.3 parts of 4,4'-diphenylmethane diisocyanate (MDI) are added, the temperature is raised to 110°C, and the reaction is carried out at a stirring speed of 450 r / min under vacuum conditions for 1 hour, and then 15 parts of modified polyurethane acrylate, 2 parts of TPO, 2.5 parts of a homemade cross-linking agent are added, 0.08 parts of a catalyst (DMDEE) are added, stirring is continued for 30 minutes, and then the material is discharged and vacuum-sealed and stored away from light.
[0039] Comparative Example 1
[0040] 24 parts of poly(hexylene adipate) diol with a molecular weight of 3500, 19 parts of poly(neopentyl adipate) diol with a molecular weight of 2000, 16 parts of polytetramethylene glycol ether diol with a molecular weight of 2000, 10 parts of acrylic resin and 5.9 parts of petroleum resin were added into a reaction bottle by weight, heated to 120-140°C, and vacuum dehydrated for 2 hours at a stirring condition of 300 / min; then, the temperature was lowered to 100°C, 13.9 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, the temperature was raised to 110°C, and the reaction was carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 0.1 parts of DMDEE were added, and the mixture was stirred at a stirring speed of 450r / min under vacuum conditions for 30 minutes, then the material was discharged, and the mixture was vacuum sealed and stored away from light.
[0041] Comparative Example 2
[0042] 20 parts of polybutylene adipate polyol with a molecular weight of 2000, 20 parts of polyoxypropylene glycol with a molecular weight of 1000, 12 parts of polyhexamethylene phthalate diol with a molecular weight of 1000, and 10 parts of petroleum resin are added to a reaction bottle by weight, heated to 120-140°C, and vacuum dehydrated for 2 hours at 350 r / min stirring conditions; then, the temperature is lowered to 100°C, 20.3 parts of 4,4'-diphenylmethane diisocyanate (MDI) are added, the temperature is raised to 110°C, and the reaction is carried out at a stirring speed of 450 r / min under vacuum conditions for 1 hour, and then 15 parts of modified polyurethane acrylate and 2 parts of TPO are added, 0.08 parts of DMDEE are added, stirring is continued for 30 minutes, and then the material is discharged and vacuum sealed for storage.
[0043] Adhesive strength test: The hot melt adhesive obtained in the embodiment and comparative example was dispensed at 110°C on a polycarbonate substrate with a width of about 2 mm using a dispensing machine. Then, another polycarbonate substrate was attached to the polycarbonate substrate, and the adhesive line was irradiated with a 365nm UV-LED light source with an irradiation energy of 10000mJ / cm 2 After the irradiation, the bonding strength was tested 2 minutes (representing the strength after light irradiation), 30 minutes, and 7 days after dispensing. The curing conditions were temperature 25°C and humidity 50% RH.
[0044] The prepared sample for evaluating the adhesive strength was stretched in the shear direction at a rate of 300 mm / min using a tensile tester to measure the shear strength with respect to the polycarbonate substrate.
[0045] The performance test results of the products obtained in Examples 1-4 and Comparative Examples are shown in Table 1.
[0046]
[0047] It can be seen from the comparative data that the polyurethane hot melt prepared by the present invention has good bonding properties immediately after UV irradiation, and also has good final bonding strength without irradiation.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A UV moisture dual-curing polyurethane hot melt adhesive, characterized in that: The synthesis steps are as follows: By weight, 24 parts of poly(hexylene adipate) diol with a molecular weight of 3500, 19 parts of poly(neopentyl adipate) diol with a molecular weight of 2000, 16 parts of polytetramethylene glycol ether diol with a molecular weight of 2000, and 5 parts of petroleum resin are added to a reaction bottle, heated to 120-140° C., and vacuum dehydrated for 2 hours at a stirring condition of 300 / min; then, the temperature is lowered to 100° C., 13.9 parts of 4,4'-diphenylmethane diisocyanate MDI are added, the temperature is raised to 110° C., and the reaction is carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 20 parts of self-made modified polyurethane acrylate, 1 part of self-made crosslinking agent, 0.1 part of catalyst DMDEE, and 1 part of photoinitiator TPO are added, and the material is stirred at a stirring speed of 450r / min for 30 minutes under vacuum conditions, and then discharged, and vacuum-sealed and light-proofed for storage; The self-made modified polyurethane acrylate is synthesized in the following steps: By weight, a mixture of 67 parts of dehydrated Bluestar Dongda EP-3600 and 2 parts of polyol pep550 was heated to 80°C, 12.9 parts of MDI were added, the temperature was raised to 100°C, and the mixture was stirred at a stirring speed of 400r / min under vacuum conditions for 1h, then the temperature was lowered to 60-80°C, 0.05 parts of p-hydroxyanisole were added, and the mixture was fully stirred, and 18 parts of caprolactone acrylate were added, the temperature was raised to 85-100°C, and the mixture was vacuumed for reaction for 2-5 hours. After the theoretical NCO content was reached, 0.05 parts of oxazolidine were added, the mixture was discharged, and the mixture was sealed and stored to obtain a homemade modified polyurethane acrylate; The self-made cross-linking agent has the following synthesis steps: By weight, 50.3 parts of multifunctional isocyanate siloxane after dehydration treatment was heated to 85°C, 0.05 parts of phenol was added and stirred evenly, 49.6 parts of caprolactone acrylate was added and heated to 85-120°C, and reacted under vacuum for 60-240 minutes. After the reaction was complete, 0.05 parts of oxazolidine was added, and the mixture was sealed and stored to obtain a homemade cross-linking agent.
2. A UV moisture dual-curing polyurethane hot melt adhesive, characterized in that: The synthesis steps are as follows: By weight, 21 parts of polyhexylene adipate diol with a molecular weight of 3500, 19 parts of polyneopentyl adipate diol with a molecular weight of 2000, 20 parts of polyoxypropylene diol with a molecular weight of 2000, and 3.8 parts of petroleum resin are added to a reaction bottle, heated to 120-140° C., and vacuum dehydrated for 2 hours at a stirring condition of 300 / min; then, the temperature is lowered to 100° C., 13.9 parts of 4,4'-diphenylmethane diisocyanate MDI are added, the temperature is raised to 110° C., and the reaction is carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 19 parts of self-made modified polyurethane acrylate, 1.5 parts of self-made crosslinking agent, 0.12 parts of catalyst DMDEE, and 1.5 parts of photoinitiator 819 are added, and the material is stirred at a stirring speed of 450r / min for 30 minutes under vacuum conditions, and then discharged, and vacuum-sealed and light-proof storage is carried out; The self-made modified polyurethane acrylate is synthesized in the following steps: By weight, a mixture of 67 parts of dehydrated Bluestar Dongda EP-3600 and 2 parts of polyol pep550 was heated to 80°C, 12.9 parts of MDI were added, the temperature was raised to 100°C, and the mixture was stirred at a stirring speed of 400r / min under vacuum conditions for 1h, then the temperature was lowered to 60-80°C, 0.05 parts of p-hydroxyanisole were added, and the mixture was fully stirred, and 18 parts of caprolactone acrylate were added, the temperature was raised to 85-100°C, and the mixture was vacuumed for reaction for 2-5 hours. After the theoretical NCO content was reached, 0.05 parts of oxazolidine were added, the mixture was discharged, and the mixture was sealed and stored to obtain a homemade modified polyurethane acrylate; The self-made cross-linking agent has the following synthesis steps: By weight, 50.3 parts of multifunctional isocyanate siloxane after dehydration treatment was heated to 85°C, 0.05 parts of phenol was added and stirred evenly, 49.6 parts of caprolactone acrylate was added and heated to 85-120°C, and reacted under vacuum for 60-240 minutes. After the reaction was complete, 0.05 parts of oxazolidine was added, and the mixture was sealed and stored to obtain a homemade cross-linking agent.
3. A UV moisture dual curing polyurethane hot melt adhesive, characterized in that: The synthesis steps are as follows: By weight, 18 parts of polyhexane adipate diol with a molecular weight of 3500, 20 parts of polycaprolactone diol with a molecular weight of 2000, 12 parts of polycarbonate diol with a molecular weight of 1000, and 2 parts of petroleum resin are added to a reaction bottle, heated to 120-140°C, and vacuum dehydrated for 2 hours at a stirring condition of 350r / min; then, the temperature is lowered to 100°C, 14.9 parts of 4,4'-diphenylmethane diisocyanate MDI are added, and the mixture is reacted at a stirring speed of 450r / min for 1 hour under vacuum conditions, and then 30 parts of self-made modified polyurethane acrylate, 2 parts of self-made crosslinking agent, 0.1 part of catalyst DMDEE, and 1 part of photoinitiator 907 are added, and the mixture is stirred at a stirring speed of 450r / min for 30 minutes under vacuum conditions, and then the material is discharged, and the mixture is vacuum sealed and stored away from light; The self-made modified polyurethane acrylate is synthesized in the following steps: By weight, a mixture of 67 parts of dehydrated Bluestar Dongda EP-3600 and 2 parts of polyol pep550 was heated to 80°C, 12.9 parts of MDI were added, the temperature was raised to 100°C, and the mixture was stirred at a stirring speed of 400r / min under vacuum conditions for 1h, then the temperature was lowered to 60-80°C, 0.05 parts of p-hydroxyanisole were added, and the mixture was fully stirred, and 18 parts of caprolactone acrylate were added, the temperature was raised to 85-100°C, and the mixture was vacuumed for reaction for 2-5 hours. After the theoretical NCO content was reached, 0.05 parts of oxazolidine were added, the mixture was discharged, and the mixture was sealed and stored to obtain a homemade modified polyurethane acrylate; The self-made cross-linking agent has the following synthesis steps: By weight, 50.3 parts of multifunctional isocyanate siloxane after dehydration treatment was heated to 85°C, 0.05 parts of phenol was added and stirred evenly, 49.6 parts of caprolactone acrylate was added and heated to 85-120°C, and reacted under vacuum for 60-240 minutes. After the reaction was complete, 0.05 parts of oxazolidine was added, and the mixture was sealed and stored to obtain a homemade cross-linking agent.
4. A UV moisture dual curing polyurethane hot melt adhesive, characterized in that: The synthesis steps are as follows: By weight, 20 parts of polybutylene adipate polyol with a molecular weight of 2000, 20 parts of polyoxypropylene glycol with a molecular weight of 1000, 12 parts of polyhexane phthalate diol with a molecular weight of 1000, and 8 parts of petroleum resin are added to a reaction bottle, heated to 130-140°C, and vacuum dehydrated for 2 hours at 350r / min stirring conditions; then, the temperature is lowered to 100°C, 20.3 parts of 4,4'-diphenylmethane diisocyanate MDI are added, the temperature is raised to 110°C, and the reaction is carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 15 parts of homemade modified polyurethane acrylate, 2 parts of photoinitiator TPO, 2.5 parts of homemade crosslinking agent are added, 0.08 parts of catalyst DMDEE are added, stirring is continued for 30 minutes, and then the material is discharged and vacuum sealed and stored away from light; The self-made modified polyurethane acrylate is synthesized in the following steps: By weight, a mixture of 67 parts of dehydrated Bluestar Dongda EP-3600 and 2 parts of polyol pep550 was heated to 80°C, 12.9 parts of MDI were added, the temperature was raised to 100°C, and the mixture was stirred at a stirring speed of 400r / min under vacuum conditions for 1h, then the temperature was lowered to 60-80°C, 0.05 parts of p-hydroxyanisole were added, and the mixture was fully stirred, and 18 parts of caprolactone acrylate were added, the temperature was raised to 85-100°C, and the mixture was vacuumed for reaction for 2-5 hours. After the theoretical NCO content was reached, 0.05 parts of oxazolidine were added, the mixture was discharged, and the mixture was sealed and stored to obtain a homemade modified polyurethane acrylate; The self-made cross-linking agent has the following synthesis steps: By weight, 50.3 parts of multifunctional isocyanate siloxane after dehydration treatment was heated to 85°C, 0.05 parts of phenol was added and stirred evenly, 49.6 parts of caprolactone acrylate was added and heated to 85-120°C, and reacted under vacuum for 60-240 minutes. After the reaction was complete, 0.05 parts of oxazolidine was added, and the mixture was sealed and stored to obtain a homemade cross-linking agent.