A reduction dyeing mother solution and its preparation method and dyeing method

By using the reduction dyeing mother liquor preparation method without insurance powder in yarn dyeing, using ammonia borane and catalyst to reduce dyeing, the problems of high pollution and treatment cost of dyeing wastewater in the prior art are solved, and efficient and environmentally friendly dyeing is achieved Effect.

CN115976857BActive Publication Date: 2024-11-08GUANGDONG FORWARD DENIM
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211693428.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-08
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The reducing dyes using insurance powder in existing yarn dyeing have problems such as poor chemical stability, excessive use and serious environmental pollution, which leads to high cost of dyeing wastewater treatment and harmful to the environment.

Method used

The reduction dyeing mother liquor preparation method is adopted without the use of insurance powder. By mixing the reducing dye and alkali liquid, the suspension is formed, ammonia borane and catalyst are added, the reaction conditions are controlled to form an active hydrogen support, and the efficient reduction dyeing mother liquor is formed, using nickel oxide. and cheap metal oxide catalysts improve the reduction rate and stability of dyes.

Benefits of technology

It significantly improves the dyeing quality, reduces hydrogen release, reduces the pollutivity of dyeing wastewater, reduces the difficulty of dyeing wastewater treatment, and improves the utilization rate and dyeing efficiency of dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
  • Figure 988735DEST_PATH_IMAGE002
    Figure 988735DEST_PATH_IMAGE002
Patent Text Reader

Abstract

The invention discloses a reduction dyeing mother liquor and a preparation method and a dyeing method thereof, which belong to the field of yarn dyeing. The reduction dyeing mother liquor preparation method comprises the following steps: mixing reduction dye and part of alkali solution to obtain reduction dye suspension; mixing ammonia borane and the remaining alkali solution to obtain active hydrogen carrier mixed solution; introducing protective gas into a reaction device to exhaust air; transferring the reduction dye suspension to the reaction device; transferring the active hydrogen carrier to the reaction device, adding a catalyst, and mixing to obtain reduction dyeing mother liquor. The reduction dyeing mother liquor has good dispersibility, strong stability, less hydrogen precipitation, and easy control of the rate and temperature of the dyeing process, which is beneficial to improving the dyeing quality. The reduction system abandons the insurance powder, is not easy to corrode the pipeline, and is beneficial to reducing the difficulty of dyeing wastewater treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a reduction dyeing mother solution and a preparation method and a dyeing method thereof, and belongs to the field of yarn dyeing. Background Art

[0002] Denim is made of white weft yarn and indigo-dyed warp yarn. Indigo is a vat dye. Most vat dyes are aromatic compounds containing carbonyl groups and do not contain water-soluble groups. Therefore, most of them are insoluble in water and need to be reduced to generate soluble leuco bodies before they can be used for yarn dyeing. At present, the industry mainly uses insurance powder to reduce and make the dye soluble. Although insurance powder has the advantages of strong reducing ability and easy use, it has poor chemical stability and reacts quickly when it comes into contact with water or encounters oxidants. It is precisely because of its poor chemical stability that the concentration of insurance powder in the dye bath drops quickly, the reduction potential loss is large, and the actual amount of insurance powder used greatly exceeds the theoretical amount. In addition, the use of insurance powder will lead to a high content of sulfites or sulfates in the wastewater, which will cause corrosion damage to the water pipeline. At the same time, the dyeing wastewater in the sewer is prone to generate toxic gases such as hydrogen sulfide, which pollutes the environment and increases the treatment cost of dyeing wastewater. Summary of the invention

[0003] In order to overcome the shortcomings of the prior art, the present invention provides a reduction dyeing mother liquor without using insurance powder, reduces the pollution of dyeing wastewater, and provides a preparation method and a dyeing method of the reduction dyeing mother liquor.

[0004] The technical solution adopted by the present invention to solve its technical problem is:

[0005] In a first aspect, the present application provides a method for preparing a reduction dyeing mother solution, comprising the following steps:

[0006] Mixing the vat dye and part of the alkali solution to obtain a vat dye suspension, and diluting with water to a solid-to-liquid ratio of the vat dye to water of 60 g / L to 180 g / L;

[0007] Mixing ammonia borane and the remaining alkali solution to obtain an active hydrogen carrier mixed solution, wherein the amount of ammonia borane used is 15%-60% of the amount of the vat dye used;

[0008] Passing protective gas into the reaction device to exhaust air;

[0009] Transferring the vat dye suspension to the reaction device and heating it to 25°C-90°C;

[0010] The active hydrogen carrier is transferred to the reaction device, a catalyst is added, and the mixture is mixed for 0.5 h to 4 h to obtain a reduction dyeing mother solution.

[0011] The method for preparing the reduction dyeing mother liquor of the present application can reduce the agglomeration of the reduction dye, make the reduction dye fully contact with ammonia borane, reduce the reduction dye with the help of a catalyst, less hydrogen is precipitated, the rate and temperature of the dyeing process are easy to control, which is beneficial to improving the dyeing quality. In addition, the method completely abandons the insurance powder, is not easy to corrode the pipeline, and is beneficial to reducing the difficulty of dyeing wastewater treatment.

[0012] Furthermore, the catalyst comprises 5%-20% of a main catalyst, 5%-10% of an auxiliary catalyst and 70%-90% of a catalyst carrier by mass, the main catalyst is nickel oxide, the auxiliary catalyst is at least one of iron oxide, copper oxide and cobalt oxide, and the catalyst carrier is γ-alumina.

[0013] Nickel oxide is used as the main catalyst, and the catalyst cost is low; other cheap metal oxides are added as co-catalysts to increase the electron density of the catalyst active sites.

[0014] Furthermore, the preparation method of the catalyst comprises:

[0015] Dissolving the nickel salt and the metal salt corresponding to the co-catalyst in deionized water to obtain an impregnation solution;

[0016] Adding γ-alumina to the impregnation solution, stirring at 60° C.-80° C. for 1 h-3 h;

[0017] Drying the impregnated γ-alumina at 100° C.-150° C. for 1 h-8 h, and then calcining at 300° C.-600° C. for 3 h-8 h to obtain the catalyst;

[0018] The amount of deionized water used is the saturated water absorption of the γ-alumina; the metal salts corresponding to the nickel salt and the co-catalyst are both nitrates or acetates.

[0019] Using γ-alumina to carry nickel oxide and other cheap metal oxides can provide multiple active sites for binding with hydroxide ions, which is more conducive to the further adsorption of active hydrogen on the catalyst surface. Metal oxides contain Lewis acid sites, which promote OH - Chemical adsorption of ions, followed by reaction of BH3 at the chemical adsorption site to form BH3(OH) - The catalyst surface has many active sites, which have moderate adsorption capacity for active hydrogen. When no dye is added, these adsorbed hydrogen are more likely to combine to form hydrogen. After adding dye, these adsorbed hydrogen are more likely to react with the dye carbonyl group, while only a small amount of gaseous hydrogen is released, and there are fewer hydrogen evolution side reactions, which significantly improves the dye reduction rate of the system.

[0020] Furthermore, the diameter of the γ-alumina is 0.5 mm-10 mm, and the BET specific surface area is 100 m 2 / g -250m2 / g.

[0021] The surface of γ-alumina of this specification has more active sites and can be easily recovered and reused after dyeing is completed.

[0022] Furthermore, the vat dye is selected from one or more of plant indigo, synthetic indigo, vat blue RSN, vat yellow G, vat green FFB, vat red FBB and the like.

[0023] Furthermore, the alkali solution is potassium hydroxide or sodium hydroxide with a mass concentration of 40%-60%. In the vat dye suspension, the amount of the alkali solution is 35%-50% of the mass of the vat dye; in the vat dyeing mother liquor, the total amount of the alkali solution is 100%-200% of the mass of the vat dye.

[0024] Furthermore, in the step of mixing the vat dye and part of the alkali solution to obtain the vat dye suspension, a wetting agent and a dispersant are also added, the wetting agent is selected from one or more of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyol ester polyoxyethylene ether, and the amount of the wetting agent is 1%-5% of the amount of the vat dye; the dispersant is selected from one or more of polymethylene dimethyl naphthalene disulfonate, naphthalene sulfonate formaldehyde condensate, sodium lignin sulfonate, styrylphenol polyoxyethylene ether sulfonate, and the amount of the dispersant is 1%-5% of the amount of the vat dye.

[0025] Before mixing with the active hydrogen carrier mixed solution, the wetting agent and the dispersant are used to further reduce the aggregation of the vat dye, so that after the active hydrogen carrier mixed solution is mixed with the vat dye suspension mixed solution, the vat dye is fully contacted with the ammonia borane.

[0026] Furthermore, the protective gas is argon or nitrogen.

[0027] In a second aspect, the present application provides a reduction dyeing mother solution, which is prepared by the method described in the first aspect, and has an oxidation-reduction potential of -850 mV to -1200 mV and a pH of 12 to 14. The reduction dyeing mother solution has good dyeing effect and strong stabilizer.

[0028] In a third aspect, the present application provides a dyeing method, comprising the following steps:

[0029] Under protective gas conditions, the reduction dyeing mother solution of the second aspect is added to the dyeing device, and water is added to dilute it to a reduction potential of -750 mV to -840 mV, a pH value of 11.5-13, and a concentration of the reduction dye of 1 g / L to 10 g / L;

[0030] The product to be dyed is placed in the dyeing device, the bath ratio is set to 1:3-20, 0.01 L / min -0.1 L / min of protective gas is continuously introduced, and dyeing is performed at the dyeing temperature.

[0031] The dyeing method can greatly reduce the pollution problem in the dyeing process, and can also significantly improve the dye reduction rate compared with the existing technology, shorten the reduction reaction time, and improve production efficiency. The dyeing effect is significantly improved compared with traditional dyeing.

[0032] The invention has the following beneficial effects: the reduction dyeing mother liquor of the invention has good dispersibility and strong stability; ammonia borane has extremely high theoretical hydrogen content; its good hydrogen release kinetics and thermodynamic properties make it a preferred material for hydrogen release by water; the reduction dye is reduced by means of a catalyst, less hydrogen is precipitated, the rate and temperature of the dyeing process are easy to control, which is beneficial to improving the dyeing quality; the reduction system abandons the insurance powder, is not easy to corrode the pipeline, and is beneficial to reducing the difficulty of dyeing wastewater treatment. DETAILED DESCRIPTION

[0033] The amount of insurance powder used is large, the chemical properties are active, and it is easy to cause environmental pollution. In recent years, people have been studying some new reduction methods, such as catalytic hydrogenation reduction. Catalytic hydrogenation reduction uses hydrogen or solid hydrogen carriers to produce active hydrogen with strong reducing properties under the action of suitable catalysts to reduce the reduction dye. Since hydrogen is flammable and explosive, it is not suitable for large-scale development in dyeing rooms, so solid hydrogen carriers are more often used. Sodium borohydride is an environmentally friendly reducing agent with a hydrogen storage capacity of 10.8% and high selectivity for ketone compounds. However, at room temperature, sodium borohydride has a slow reduction rate and poor efficiency for reducing dyes, so a specific reducing agent and a higher temperature are required, which makes the reduction process complicated and the reaction controllability is poor.

[0034] In order to solve the problems of high catalyst cost, poor activity, low selectivity, complex reduction process, high reaction temperature, high energy consumption, poor controllability, low reduction efficiency and poor dyeing quality in the catalytic hydrogenation reduction reaction of reduced dyes, the present invention provides a method for preparing a reduced dyeing mother solution, comprising the following steps:

[0035] S1: Mix the vat dye and part of the alkali solution to obtain a vat dye suspension, and dilute it with water to a solid-to-liquid ratio of 60 g / L to 180 g / L.

[0036] S2: Mix ammonia borane and the remaining alkali solution to obtain an active hydrogen carrier mixed solution, wherein the amount of ammonia borane used is 15%-60% of the amount of the vat dye used.

[0037] S3: Introduce protective gas into the reaction device to exhaust air.

[0038] S4: Transfer the reduced dye suspension to a reaction device and heat it to 25°C-90°C.

[0039] S5: The active hydrogen carrier is transferred to a reaction device, a catalyst is added, and the mixture is mixed for 0.5 h to 4 h to obtain a reduction dyeing mother solution.

[0040] The redox potential of the resulting reduction dyeing solution is -850 mV to -1200 mV, and the pH is 12-14.

[0041] The present application first prepares a reduced dye suspension and an active hydrogen carrier mixed liquid. The two liquids are relatively stable and easy to store when not mixed. When used, they are mixed into a reduced dyeing mother liquid and placed in a mother liquid tank of a dye vat. The reduced dye is continuously reduced to a soluble substance by ammonia borane, and does not react violently like insurance powder to release a large amount of heat. It has strong controllability, a relatively stable reduction potential, and can continuously and efficiently act.

[0042] The vat dye is selected from one or more of plant indigo, synthetic indigo, vat blue RSN, vat yellow G, vat green FFB, vat red FBB, etc. The alkali solution is potassium hydroxide or sodium hydroxide, with a mass concentration of 40%-60%. In the vat dye suspension, the amount of the alkali solution is 35%-50% of the mass of the vat dye; in the vat dyeing mother liquor, the total amount of the alkali solution is 100%-200% of the vat dye.

[0043] Vat dyes are easy to agglomerate, and the preparation method of the present invention can make the system have better dispersibility, which is conducive to full contact between various substances and high reaction efficiency.

[0044] Preferably, in the step of mixing the vat dye and part of the alkali solution to obtain the vat dye suspension, a wetting agent and a dispersant are also added, the wetting agent is selected from one or more of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyol ester polyoxyethylene ether, and the amount of the wetting agent is 1%-5% of the amount of the vat dye; the dispersant is selected from one or more of polymethylene dimethyl naphthalene disulfonate, naphthalene sulfonate formaldehyde condensate, sodium lignin sulfonate, styrylphenol polyoxyethylene ether sulfonate, and the amount of the dispersant is 1%-5% of the amount of the vat dye. Before mixing with the active hydrogen carrier mixed solution, the wetting agent and the dispersant are used to further reduce the aggregation of the vat dye, so that after the active hydrogen carrier mixed solution is mixed with the vat dye suspension mixed solution, the vat dye is fully contacted with the ammonia borane.

[0045] The catalyst comprises 5%-20% of a main catalyst, 5%-10% of an auxiliary catalyst and 70%-90% of a catalyst carrier by mass. The main catalyst is nickel oxide, the auxiliary catalyst is at least one of iron oxide, copper oxide and cobalt oxide, and the catalyst carrier is γ-alumina.

[0046] Nickel oxide is used as the main catalyst, and the catalyst cost is low; other cheap metal oxides are added as co-catalysts to increase the electron density of the catalyst active sites.

[0047] The preparation method of the catalyst comprises:

[0048] Dissolving the nickel salt and the metal salt corresponding to the co-catalyst in deionized water to obtain an impregnation solution;

[0049] Add γ-alumina to the impregnation solution and stir at 60-80°C for 1-3 h;

[0050] Drying the impregnated γ-alumina at 100° C.-150° C. for 1 h-8 h, and then calcining at 300° C.-600° C. for 3 h-8 h to obtain a catalyst;

[0051] The amount of deionized water used is the saturated water absorption of γ-alumina; the metal salts corresponding to the nickel salt and the cocatalyst are all nitrates or acetates. For example, when nickel acetate is used as the nickel salt, the metal salt corresponding to the cocatalyst should be ferric acetate, cobalt acetate, etc. The diameter of γ-alumina is 0.5 mm-10 mm, and the BET specific surface area is 100 m 2 / g -250 m 2 / g.

[0052] The present invention uses ammonia borane with a very high theoretical hydrogen content (19.6%) as a hydrogen carrier and nickel oxide as a main catalyst to effectively reduce the catalyst cost; a co-catalyst is added as an activator to increase the electron density of the catalyst active site; the metal oxide contains an activator metal with Lewis acid sites to promote OH - Chemical adsorption of ions, followed by reaction of BH3 at the chemical adsorption site to form BH3(OH) - . The catalyst surface has a large number of active sites, which have moderate adsorption capacity for active hydrogen. When no dye is added, these adsorbed hydrogen are easier to combine to form hydrogen. After the dye is added, these adsorbed hydrogen are easier to react with the dye carbonyl. In addition, the active sites make the dye carbonyl activated, which makes it easier to react with active hydrogen to complete hydrogenation reduction. At the same time, only a small amount of gaseous hydrogen is released, and there are few hydrogen evolution side reactions, which significantly improves the dye reduction rate of the system. The catalyst is a small spherical metal oxide, which is easy to recycle and reuse. When this system is used for reduction dyeing of reduction dyes, the use of insurance powder is completely abandoned. The reduction process is cleaner and more environmentally friendly, and the biocompatibility of wastewater is good, which greatly reduces the cost of wastewater treatment.

[0053] The present application also provides a method for using a reduction dyeing mother solution, comprising the following steps:

[0054] Under protective gas conditions, the reduction dyeing mother solution of the second aspect is added to the dyeing device, and water is added to dilute it to a reduction potential of -750 mV to -840 mV, a pH value of 11.5-13, and a concentration of the reduction dye of 1 g / L to 10 g / L;

[0055] Place the product to be dyed into the dyeing device, set the bath ratio to 1:3-20, continuously introduce 0.01 L / min -0.1L / min of protective gas, and dye at the dyeing temperature. The protective gas is argon or nitrogen. The dyeing temperature refers to the conventional dyeing temperature of the selected reducing dye, which is generally 25℃-90℃. The dyeing time is 10 min -120min. The cotton product to be dyed can be cotton fabric, cotton yarn, cotton blended fabric, cotton blended yarn or denim fabric. Leveling agent, dye accelerator and penetrant can be added during the dyeing process, or no leveling agent, dye accelerator and penetrant can be added. The oxidation conditions are air oxidation or oxidant oxidation at room temperature, and the air oxidation time can be 5 minutes-30 minutes; oxidant oxidation can be oxidized with 5 g / L hydrogen peroxide (30% mass percent hydrogen peroxide) at 30℃ for 5 min-30 min.

[0056] Specifically, the steps before dyeing also include pretreatment and a first water wash, and the steps after dyeing also include oxidation, soaping, a second water wash, and drying.

[0057] The pretreatment conditions include: the pH of the active oxygen pretreatment solution is 6-8, the temperature of the treatment solution is 10°C-30°C, the bath ratio is 1:5 to 1:30, and an active oxygen generator is used in the pretreatment tank to pass ozone into the aqueous solution in the pretreatment tank to form an ozone aqueous solution with an ozone concentration of 50 mg / L-200 mg / L, and the treatment time is 5 min-30 min.

[0058] For soap washing, use 4 g / L soap powder and 3 g / L sodium carbonate, boil the soap at 93±2℃ for 20 min, and the bath ratio is 1:50.

[0059] Example 1

[0060] Preparation of nickel-based alumina catalyst: The diameter of the catalyst was 0.5 mm and the specific surface area was 150 m 2 / g of 10g γ-Al2O3 carrier was dried at 80℃ for 3h, then 2.48g nickel nitrate and 1.49g copper nitrate were taken in a beaker, water was added to 10mL, and the mixture was thoroughly stirred. The dried alumina carrier was further added to the impregnation solution, impregnated at 60℃ for 2h under stirring conditions, dried at 130℃ for 4h, and finally calcined at 450℃ for 4h to obtain a nickel-based alumina catalyst (nickel oxide content: 15%, copper oxide content: 7%, alumina content: 78%).

[0061] Preparation of reduction dyeing mother liquor: Add 80 g of indigo dye and 40 g of 50% NaOH solution, 2 g of wetting agent (fatty alcohol polyoxyethylene ether), and 2 g of dispersant (sodium polymethylene dimethyl naphthalene disulfonate) to 1L of distilled water and mix thoroughly to obtain a reduction dye suspension. Fully mix 20 g of ammonia borane and 100 g of 50% alkali solution to obtain an active hydrogen carrier mixed solution. Pass nitrogen into the reaction device to exhaust the air inside. Transfer the reduction dye suspension to the reduction reaction device and heat it to 50°C. Transfer the active hydrogen carrier to the reaction container, mix thoroughly, add the nickel-based alumina catalyst, stir continuously, and react for 2 h to obtain a reduction dyeing mother liquor.

[0062] Dyeing: Take 5g of cotton fabric pretreated with active oxygen, set the bath ratio to 1:20, add 2.5mL of the above reduction dyeing mother solution into the dyeing device, add water to dissolve to 100mL, and dye at room temperature (28℃) for 20min. During this period, nitrogen was continuously introduced into the dyeing device, the nitrogen flux was 0.05 L / min, the dye solution reduction potential was tested to be -820mV, and the pH value was 12.7. Before dyeing, 5g of cotton fabric to be dyed was pretreated with active oxygen (bath ratio 1:20, treatment temperature 30℃, treatment solution pH value 7, ozone concentration 50 mg / L, treatment time 15 min), and then washed for the first time. After dyeing, oxidation (air oxidation for 20 min), soap washing (soap washing is soap powder 4 g / L, sodium carbonate 3 g / L, 93±2℃ soap boiling for 20 min, bath ratio 1:50), second washing, and drying.

[0063] Finally, the dyed fabric is taken to test its color fastness and dyeing K / S value, and the COD and BOD of the dyeing residual liquid are tested.

[0064] Comparative Example 1

[0065] Reduction: first add 80 g of indigo, 160 g of hydrosulfite and 100 g of caustic soda into 1 L of distilled water and carry out pre-reduction treatment at 60 °C for 2 h to obtain reduction dyeing mother liquor.

[0066] Dyeing: Under room temperature, take 5g of cotton fabric pretreated with active oxygen, set the bath ratio to 1:20, add 2.5mL of the above reduction dyeing mother solution to the dyeing device, dilute with water to 100mL, dye for 20min, test the dye solution reduction potential -788mV, pH value is 13. Before dyeing, 5g of cotton fabric to be dyed is pretreated with active oxygen (bath ratio 1:20, treatment temperature 30℃, treatment solution pH value 7, ozone concentration 50mg / L, treatment time 15min), and then washed for the first time. After dyeing, oxidation (air oxidation for 20min), soap washing (soap washing is 4g / L soap powder, 3g / L sodium carbonate, 93±2℃ soap boiling for 20min, bath ratio 1:50), second washing, and drying.

[0067] Finally, the dyed fabric is taken to test its color fastness and dyeing K / S value, and the COD and BOD of the dyeing residual liquid are tested.

[0068] Comparative Example 2

[0069] Reduction: Add 80 g of indigo dye, 60 g of sodium borohydride, and 80 g of caustic soda to 1 L of distilled water at 55 °C for pre-reduction treatment for 2 h.

[0070] Dyeing: Under room temperature, take 5g of cotton fabric pretreated with active oxygen, set the bath ratio to 1:20, add 2.5mL of the above reduction dyeing mother solution to the dyeing device, dilute with water to 100mL, dye for 20min, test the dye solution reduction potential -720mV, pH value is 12.5. Before dyeing, 5g of cotton fabric to be dyed is pretreated with active oxygen (bath ratio 1:20, treatment temperature 30℃, treatment solution pH value 7, ozone concentration 50mg / L, treatment time 15min), and then washed for the first time. After dyeing, oxidation (air oxidation for 20min), soap washing (soap washing is soap powder 4g / L, sodium carbonate 3g / L, 93±2℃ soap boiling for 20min, bath ratio 1:50), washing, and drying are carried out.

[0071] Finally, the dyed fabric is taken to test its color fastness and dyeing K / S value, and the COD and BOD of the dyeing residual liquid are tested.

[0072] Test description:

[0073] Measurement of reduction potential: Refer to the industry standard "SL94-1994 Determination of Redox Potential", use a redox potentiometer, place the reduction potentiometer in the dye solution at room temperature, and read the reduction potential value after the value stabilizes.

[0074] K / S value: Fold the sample into 4 layers (opaque) and use Color-i5 computer colorimeter (X-Rite, USA) to test. Measure 3 different locations and take the average value.

[0075] Fabric rubbing fastness test: refer to "GB / T 3920-2008 Textiles Color Fastness Test-Rubbing Color Fastness" using Y571-Ⅱ Color Fastness Friction Tester. Measure 3 times and take the average value.

[0076] Absorbance: The JH756 UV-visible spectrophotometer was used to measure the absorbance value at the maximum absorption wavelength of the dye wastewater (indigo 670nm). The greater the absorbance, the more indigo dye is left in the wastewater. Under the same dye dosage, the greater the absorbance of the wastewater at 670nm, the lower the dye utilization rate of the process.

[0077] Dilute dye solution BOD test: refer to "HJ / T86-2002 Rapid determination method of water quality biochemical oxygen demand by microbial sensor", measure each group of dye solution 3 times and take the average value.

[0078] Dilute dye liquor COD test: refer to "HJ / T399-2007 Rapid Determination of Chemical Oxygen Demand of Water Quality - Rapid Digestion Spectrophotometry", first digest each group of dye liquor in the digester for 10 minutes, then measure the dye liquor COD three times and take the average value.

[0079] The fabrics obtained in the examples and comparative examples were tested for various properties. The dyeing results are shown in Table 1, and the test results of the biodegradability of the dye solution are shown in Table 2.

[0080] Table 1

[0081]

[0082] It can be seen from the above embodiments and comparative examples that the dyed fabric obtained by the dyeing method of the present invention has a greatly improved K / S value and color fastness compared with the prior art, and has a good dyeing effect.

[0083] Table 2

[0084]

[0085] The biodegradability of dyeing residual liquid refers to the degree to which the pollutants contained in the dyeing residual liquid are biodegradable. The BOD / COD (B / C) ratio method is often used as a measure of biodegradability. Dyeing residual liquid with B / C>0.3 is a biodegradable residual liquid. The higher the B / C, the better the effect of aerobic biological treatment of the dyeing residual liquid. As can be seen from Table 2, the COD and BOD of the indigo dyeing liquid after reduction dyeing using this technology are lower than those of traditional insurance powder reduction and sodium borohydride catalytic hydrogenation reduction dyeing, and the B / C is higher. This shows that the dyeing liquid after the indigo reduction dyeing of the invention is easier to chemically and biologically degrade, which can greatly reduce the BOD and COD values ​​of the dyeing wastewater, reduce the burden of wastewater treatment, and has obvious environmental benefits. The wastewater has a lower absorbance to 670nm light, and the dye utilization rate of this process is higher.

[0086] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a reduction dyeing mother solution, characterized in that: The following steps are involved: Mixing the vat dye and part of the alkali solution to obtain a vat dye suspension, and diluting with water to a solid-to-liquid ratio of the vat dye to water of 60 g / L to 180 g / L; Mixing ammonia borane and the remaining alkali solution to obtain an active hydrogen carrier mixed solution, wherein the amount of ammonia borane used is 15%-60% of the amount of the vat dye used; Passing protective gas into the reaction device to exhaust air; Transferring the vat dye suspension to the reaction device and heating it to 25°C-90°C; The active hydrogen carrier is transferred to the reaction device, a catalyst is added, and mixed for 0.5 h-4 h to obtain a reduction dyeing mother solution; The catalyst comprises 5%-20% of a main catalyst, 5%-10% of an auxiliary catalyst and 70%-90% of a catalyst carrier by mass, the main catalyst is nickel oxide, the auxiliary catalyst is at least one of iron oxide, copper oxide and cobalt oxide, and the catalyst carrier is γ-alumina.

2. The method for preparing a reduction dyeing mother solution according to claim 1, wherein: The preparation method of the catalyst comprises: Dissolving the nickel salt and the metal salt corresponding to the co-catalyst in deionized water to obtain an impregnation solution; Adding γ-alumina to the impregnation solution, stirring at 60° C.-80° C. for 1 h-3 h; Drying the impregnated γ-alumina at 100° C.-150° C. for 1 h-8 h, and then calcining at 300° C.-600° C. for 3 h-8 h to obtain the catalyst; The amount of deionized water used is the saturated water absorption of the γ-alumina; the metal salts corresponding to the nickel salt and the co-catalyst are both nitrates or acetates.

3. The method for preparing a reduction dyeing mother solution according to claim 2, wherein: The diameter of the γ-alumina is 0.5 mm-10 mm, and the BET specific surface area is 100 m 2 / g -250 m 2 / g.

4. The method for preparing a reduction dyeing mother solution according to claim 1, wherein: The vat dye is selected from one or more of plant indigo, synthetic indigo, vat blue RSN, vat yellow G, vat green FFB, vat red FBB and the like.

5. The method for preparing a reduction dyeing mother solution according to claim 1, wherein: The alkali solution is potassium hydroxide or sodium hydroxide with a mass concentration of 40%-60%. In the vat dye suspension, the amount of the alkali solution is 35%-50% of the mass of the vat dye; in the vat dyeing mother liquor, the total amount of the alkali solution is 100%-200% of the mass of the vat dye.

6. The method for preparing a reduction dyeing mother solution according to claim 1, characterized in that: In the step of mixing the vat dye and part of the alkali solution to obtain the vat dye suspension, a wetting agent and a dispersant are also added, wherein the wetting agent is selected from one or more of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyol ester polyoxyethylene ether, and the amount of the wetting agent is 1%-5% of the amount of the vat dye; the dispersant is selected from one or more of polymethylene dimethyl naphthalene disulfonate, naphthalene sulfonate formaldehyde condensate, sodium lignin sulfonate, and styrylphenol polyoxyethylene ether sulfonate, and the amount of the dispersant is 1%-5% of the amount of the vat dye.

7. The method for preparing a reduction dyeing mother solution according to claim 1, characterized in that: The protective gas is argon or nitrogen.

8. A reduction dyeing mother liquor, characterized in that: Prepared by the method according to any one of claims 1 to 7, the redox potential is -850 mV to -1200 mV, and the pH is 12-14.

9. A dyeing method, characterized in that: The following steps are involved: Under protective gas conditions, the reduction dyeing mother solution as claimed in claim 8 is added to a dyeing device, and water is added to dilute it to a reduction potential of -750 mV to -840 mV, a pH value of 11.5-13, and a concentration of the reduction dye of 1 g / L to 10 g / L; The product to be dyed is placed in the dyeing device, the bath ratio is set to 1:3-20, 0.01 L / min-0.1 L / min of protective gas is continuously introduced, and dyeing is performed at the dyeing temperature.

Citation Information

Patent Citations

  • Indigo dye reducing liquid as well as preparation method and production device thereof

    CN113717542A

  • Improvements in the Manufacture of Leuco-derivatives of Vat Dye-stuffs.

    GB191419848A