A method for measuring residual stress distributed locally along the layer depth of metal composite plates
By combining electrolytic stripping technology with X-ray diffraction method, the problem of limited measurement depth of X-ray diffraction method is solved, and residual stress measurement in a wide range of depths of metal composite plates is achieved, ensuring measurement accuracy and protection of material properties. It is suitable for A variety of composite panel materials.
Patent Information
- Application Number
- CN202310036926.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-10
AI Technical Summary
The existing X-ray diffraction method can only measure the residual stress distribution within 20 μm on the surface of the metal composite plate, and the mechanical delamination method will destroy the original shape of the material and introduce external stress, making it difficult to measure the residual stress inside the deeper composite plate.
Using electrolytic stripping method combined with X-ray diffraction method, by designing a special glass cup and electrolytic corrosion device, the metal composite plate is corroded layer by layer, and the corrosion depth is controlled to reach 2mm. The residual stress at the surface, far interface, near interface and interface is measured. Avoid large-area damage and external stress.
It achieves residual stress measurement of metal composite panels with a large depth and wide range, ensuring the accuracy of measurement results and protection of material properties. It is suitable for a variety of metal composite panel materials, is easy to operate, low-cost, and efficient.
Smart Images

Figure CN115979478B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material residual stress testing, and in particular relates to an electrolytic stripping method for measuring the residual stress distributed locally along the layer depth of a metal composite plate based on an X-ray diffraction method. Background Art
[0002] Metal composite plates have been widely used in aviation, petroleum, chemical industry, shipbuilding and other industrial fields due to their excellent comprehensive mechanical properties. However, during the rolling process of composite plates, the base material and the covering material have different mechanical and physical properties, which results in large residual stress in the composite plates due to the incoordination of the deformation of dissimilar metals. The generation of residual stress will cause the plate to warp and deform, and cracks to form at the composite interface, and will also affect the subsequent processing and performance of the composite plates. Therefore, in order to study the distribution law of residual stress in composite plates and regulate the spatial and temporal distribution of residual stress inside composite plates, accurate measurement of residual stress in composite plates is particularly critical.
[0003] At present, the commonly used residual stress detection methods are mainly divided into two categories: non-destructive testing and destructive testing. Non-destructive testing technologies include X-ray diffraction, neutron diffraction, magnetic measurement, ultrasonic method and other methods; destructive testing technologies include drilling method and cutting method. Compared with other methods, the X-ray diffraction method in non-destructive testing has the advantages of mature technology and high measurement accuracy, but the X-ray diffraction method can only measure the residual stress distribution within 20μm on the surface of the material. Patent No. CN202110557213.4 "A residual stress test method for steel thin welding plate with narrow weld characteristics" uses electrolytic polishing layer-by-layer peeling technology and X-ray diffraction to measure the magnitude and direction of residual stress at the grinding depth of narrow welds. However, this mechanical peeling method will destroy the original residual stress state of the material over a large area, introduce external residual stress into the material, and affect the accuracy of the measurement results. Patent No. CN200910213023.X "A device and method for controlling residual stress on the surface of a metal microstructure through a laser micro-shot peening device" uses X-ray diffraction to measure residual stress on the metal surface in the range of 100 to 200 μm. Patent No. CN202010083066.7 "A residual stress test method for additive products" realizes the stripping of the product surface by controlling the electrolytic corrosion method, and then measures the surface residual stress by the X-ray diffraction method, but the corrosion depth is also limited to 200 to 300 μm. Therefore, in order to measure the residual stress inside the material with controllable depth and without introducing external residual stress, an electrolytic stripping method based on X-ray diffraction can be used to achieve this. However, metal composite plates often need to measure residual stress at multiple depths such as the surface, far interface, near interface, and interface. The measurement depth is deep, and it is necessary to measure without destroying the original residual stress. Summary of the invention
[0004] In view of the problem that the X-ray diffraction method can only measure the residual stress on the surface of the material, the present invention proposes a method for measuring the residual stress distributed locally along the layer depth of a metal composite plate. The corrosion depth can reach up to 2mm, which meets the requirements of large depth and wide range of metal composite plate measurement. While avoiding large-area peeling and not destroying the material properties and original residual stress, the residual stress on the surface, far interface, near interface and interface of the composite plate can be measured.
[0005] The technical means adopted by the present invention are as follows:
[0006] A method for measuring residual stress distributed locally along the layer depth of a metal composite plate comprises the following steps:
[0007] S1. Surface treatment: Grind and clean the surface of the metal composite plate, and try to ensure that the measuring position is flat, and then wipe the surface clean with alcohol; experiments have shown that the surface quality of the material after corrosion is closely related to the surface quality before corrosion, and it should be ensured that there is no stain on the surface of the material before corrosion;
[0008] S2. Paste the glass cup: Select the measurement position in a distributed manner along the rolling direction and transverse direction of the metal composite plate, and then paste one or more glass cups with through holes at the bottom to the measurement position. The through holes at the bottom of the glass cup should be tightly pasted to the metal composite plate without any gaps to ensure that the electrolyte will not leak from the gaps at the bottom of the cup during the corrosion process. The through holes at the bottom of the glass cup should be aligned with the measurement point, and then wait for the glue to dry;
[0009] S3. Electrolytic corrosion: Since the measurement depth of the X-ray diffraction method is limited, in order to obtain stress results at different depths, and at the same time, no residual stress can be added during the sample processing, the electrolytic corrosion stripping method is selected. The specific operations include: the device used in the electrolytic corrosion stripping method is composed of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material; add an electrolyte to a depth of two-thirds into the glass cup attached to the metal composite plate, the electrolyte is a saturated NaCl solution, and then connect one end of the graphite rod to one end of the negative electrode, insert the other end of the graphite rod into the electrolyte in the glass cup, and the other end of the negative electrode is connected to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the test material, and the other end is connected to the positive electrode of the voltage-stabilized power supply through a wire; the power supply device is used to perform local electrolytic stripping of the metal composite plate at the through hole at the bottom of the glass cup layer by layer; specifically, the electrochemical reaction between the positive and negative electrodes of the power supply, the electrolyte and the metal to be corroded is used to achieve local electrolytic stripping of the metal composite plate to be tested connected to the positive electrode;
[0010] S4. Corrosion depth measurement: ensure that the corrosion current remains unchanged, change the corrosion time, measure the corrosion depth at different corrosion times (keep the diameter of the through hole at the bottom of the glass the same), and obtain the variation law of the corrosion depth of the corroded material with the corrosion time;
[0011] S5, stress detection: measure each corrosion position, and ensure that the measurement position and direction of the metal composite plate remain consistent during each measurement; then loop through steps S2 to S5 until the corrosion depth reaches the required depth and the stress detection is completed.
[0012] The above-mentioned method for measuring the residual stress distributed locally along the layer depth of a metal composite plate, wherein:
[0013] In the step S1, the surface treatment of the metal composite plate is carried out by ultrasonic cleaning, mechanical grinding and pickling to remove rust and oil stains on the surface, as well as high-pressure cleaning and drying.
[0014] In step S2, the glass is a special glass with an inner diameter of 30-50 mm, a height of 30-50 mm, a wall thickness of 1-5 mm, a bottom through hole diameter of 4-12 mm, and the through hole is arranged at the center of the bottom of the glass. The diameter of the through hole at the bottom of the special glass is designed according to the target depth to be corroded. The smaller the diameter, the deeper the corrosion depth. The corrosion depth has a certain electrochemical relationship with the size of the corrosion area. The glass can also be replaced with other transparent materials that are not conductive and will not participate in electrochemical reactions during the electrolytic corrosion process.
[0015] In the step S2, according to the demand for the number of test point positions of the metal composite plate, the sticking positions of the glass cups are distributedly designed along the rolling direction and the transverse direction of the composite plate. The rolling direction refers to the rolling direction of the metal composite plate, and the transverse direction refers to the direction perpendicular to the rolling direction. The number of the glass cups can be single or several. The specific number is determined by the number of positions to be corroded. Preferably, the number of glass cups is less than or equal to 5. The method of "waiting for the glue to dry" can be selected to dry at room temperature, or it can be accelerated by heating and blowing. The thickness of the glue between the bottom of the glass cup and the metal plate should be controlled as much as possible while ensuring uniform application. The thickness should not be too thick to avoid affecting the corrosion process.
[0016] In step S5, the parameters of the X-ray stress tester are as follows: the X-ray wavelength is determined according to the selected target material, the residual stress of the composite plate is measured by the tilt method, the measurement start angle is 150-154°, the end angle is 155-160°, the measurement step width is 0.04°, and the test time of each step width is 0.1-0.3s; at this time, the DST-177 high-resolution X-ray stress tester sets the measurement tube voltage to 10-25kV and the tube current to 5-40mA. The parameters of the above X-ray stress tester can be appropriately adjusted according to different corroded metal materials.
[0017] Compared with the prior art, the method of the present invention obtains the residual stress distribution law of the material in the depth direction by corroding the metal composite plate locally layer by layer, thereby solving the problem that the X-ray diffraction method can only measure the residual stress on the surface of the material. By controlling the corrosion time, the corrosion depth can be accurately controlled, and the surface quality of the small holes after corrosion is good, so the purpose of accurately measuring the residual stress size at different depths of the local metal composite plate can be achieved. By measuring the residual stress inside the composite plate, relevant processes can be formulated to reduce or eliminate the internal residual stress, and the electrolytic stripping method can be closely coordinated with it to achieve the control of the residual stress inside the metal composite plate, which provides a strong guarantee for improving the subsequent processing and use performance of the metal composite plate.
[0018] The present invention has the following advantages:
[0019] 1. The X-ray diffraction method can only measure the residual stress within 20 μm of the material surface. Combined with the electrolytic stripping method of the present invention, the residual stress of the metal composite plate at various depths within 2 mm from the surface can be measured.
[0020] 2. By designing a special corrosion-assisted glass cup, single-point or multi-point corrosion with a fixed diameter and depth at specific positions distributed along the rolling and transverse directions of the composite plate can be completed. On the premise of determining the diameter of the through hole at the bottom of the glass cup, precise control of the corrosion depth can be achieved by controlling the corrosion time and current.
[0021] 3. Through experimental tests, the surface of the small holes after electrolytic stripping is smooth and flat, which fully meets the measurement requirements of the X-ray diffraction method for the material surface and ensures the accuracy of the measurement results.
[0022] 4. The method of the present invention has a small peeling area and a wide range of applications. It can measure not only small samples, but also specific local areas of large workpieces, and is applicable to a variety of metal composite plate materials. In addition, the method of the present invention has little damage to the material and can avoid the influence of large-area peeling on material properties and original residual stress. The influence of the method of the present invention on the original residual stress of the workpiece can be ignored.
[0023] 5. In the whole experimental process, the test device is simple to prepare, the operation process is convenient, the cost is low, the efficiency is high, the experimental cycle is short, the repeatability is strong, and it can corrode to the required measurement position quickly and accurately.
[0024] 6. When the corrosion current remains unchanged, the corrosion depth at the detection position of the metal composite plate can be determined according to the diameter of the through hole at the bottom of the glass cup and the length of the corrosion time, and finally the residual stress at the surface, far interface, near interface and interface of the metal composite plate can be measured. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of the electrolytic stripping experimental device of the present invention;
[0026] Figure 2 This is a graph showing the corresponding relationship between the corrosion depth and corrosion time of steel materials obtained by experimental measurement at a current of 1A;
[0027] Figure 3 This is a surface photo of the corrosion pit of the present invention after corrosion for 10 minutes;
[0028] Figure 4 This is a microscopic photo of the corrosion pits of the present invention after corrosion for 10 minutes;
[0029] Figure 5 This is a surface photo of the corrosion pit of the present invention after corrosion for 20 minutes;
[0030] Figure 6 This is a microscopic photo of the corrosion pits of the present invention after 20 minutes of corrosion;
[0031] Figure 7 This is a surface photo of the corrosion pit of the present invention after corrosion for 30 minutes;
[0032] Figure 8 This is a microscopic photograph of the corrosion pits of the present invention after corrosion for 30 minutes;
[0033] Fig. 9 Trend diagram of depth and stress distribution along the layer depth;
[0034] Fig.10 This is a microscopic photo of the corrosion pit of the present invention at a current of 2A and corrosion for 25 minutes;
[0035] Fig.11 This is a microscopic photograph of the corrosion pits of the present invention at a current of 2A and corrosion for 40 minutes. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are embodiments of a part of the present invention, not all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0037] like Figure 1 As shown, a method for measuring residual stress distributed locally along the layer depth of a metal composite plate comprises the following steps:
[0038] S1. Surface treatment: Grind and clean the surface of the composite board, and try to ensure that the measuring position is flat, then wipe the surface with alcohol, and try to ensure that there is no stain on the surface of the material before corrosion;
[0039] S2. Paste the glass cup: Select the measurement position along the rolling direction and transverse direction of the metal composite plate, apply glue evenly on the bottom of the glass cup, and then paste one or more glass cups with through holes on the bottom to the measurement position, so that the space between the bottom of the glass cup and the material is filled with glue, and the area around the through hole and the material are tightly glued together with no gaps. Align the through hole at the bottom of the cup with the measurement point, and then wait for the glue to dry, so that the glass cup and the material are tightly combined to ensure that the electrolyte will not leak from the bottom of the cup during the corrosion process;
[0040] S3. Electrolytic corrosion: The measurement depth of the X-ray diffraction method is limited. In order to obtain stress results at different depths and not add any residual stress during the sample processing, the electrolytic corrosion stripping method is selected. The specific operation is as follows: The main parts of the device used for electrolytic corrosion stripping are composed of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material; add two-thirds of the depth of electrolyte into the glass cup pasted on the metal composite plate, and the electrolyte is a saturated NaCl solution. Then connect one end of the graphite rod to one end of the negative electrode, insert the other end of the graphite rod into the electrolyte in the glass cup, and the other end of the negative electrode is connected to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the measured material, and the other end is connected to the positive electrode of the voltage-stabilized power supply through a wire. Use the power supply device to perform local electrolytic stripping of the metal composite plate at the through hole at the bottom of the glass cup layer by layer; use the positive and negative electrodes of the power supply, the electrochemical reaction between the electrolyte and the metal to be corroded, to achieve local electrolytic stripping of the measured position of the metal composite plate connected to the positive electrode;
[0041] S4. Corrosion depth measurement: Keep the corrosion current constant and change the corrosion time. Since the diameter of the through hole at the bottom of the designed glass cup is the same, the corrosion depth at different corrosion times can be measured to obtain the variation law of the corrosion depth of the corroded material with the corrosion time. Finally, the corrosion depth can be determined by setting the corrosion time.
[0042] S5. Stress detection: Use XSTRESS DST-17 stress meter to measure each corrosion position. The wavelength of X-ray is determined according to the selected target material, and the residual stress of the composite plate is measured by the tilt method. The starting angle of measurement is 150-154°, the ending angle is 155-160°, the measurement step width is 0.04°, and the test time for each step width is 0.1-0.3s; at this time, the DST-177 high-resolution X-ray stress meter sets the measurement tube voltage to 10-25kV and the tube current to 5-40mA. The parameters of the above X-ray stress meter can be appropriately adjusted according to the different corroded metal materials.
[0043] During each measurement, the measurement position and direction of the composite plate are ensured to be consistent; then steps S2 to S5 are looped until the corrosion depth reaches the required depth and the stress detection is completed.
[0044] Example 1
[0045] In this example, a composite plate with 316 stainless steel as the cladding material and Q345 as the substrate is rolled. After rolling, the residual stress distribution within the range of 0.97 mm from the surface position to the interface position on the 316 stainless steel side of the composite plate is measured using the method of the present invention. This example mainly studies the variation law of the residual stress on the 316 stainless steel side within the depth range, so the experimental steps are all carried out on the 316 stainless steel side. The specific operation steps are as follows:
[0046] S1. Surface treatment: First, clean the iron oxide on the side surface of the composite plate 316 stainless steel, then polish it with 1000-grit sandpaper, and then wipe the surface repeatedly with acetone until all the stains on the surface are cleaned.
[0047] S2. Paste the glass cup: Select the measurement position along the rolling direction and transverse direction of the metal composite plate, and take 2 special glass cups with an inner diameter of 30mm and a bottom through hole of 7mm. The through hole is set at the center of the bottom of the cup, 30mm high and 1mm thick. Then apply glue evenly on the bottom of the glass cup, paste the glass cups on the stainless steel surface respectively, and align the through hole with the measurement position. During this process, rotate the glass cup around the center to ensure that there is glue between the glass cup and the stainless steel without gaps. During this process, it should be ensured that the stainless steel surface at the through hole position is not stained with glue to avoid affecting the corrosion effect. Wait until the glue is dry and the glass cup is firmly attached to the stainless steel side.
[0048] S3, electrolytic corrosion: The electrolytic corrosion stripping method is selected. The device used for electrolytic corrosion stripping consists of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material. The specific operation is as follows: add two-thirds of the depth of electrolyte to the glass cup attached to the metal composite plate. The electrolyte is a saturated NaCl solution, and then connect one end of the graphite rod to one end of the negative electrode, insert the other end of the graphite rod into the electrolyte in the glass cup 4-5mm, and connect the other end of the negative electrode to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the measured material, and the other end is connected to the positive electrode of the voltage-stabilized power supply through a wire. After checking the circuit path, start the power switch, adjust the current to stabilize at 1A, and then start timing.
[0049] S4. Corrosion depth measurement: Through experiments, the corresponding relationship between corrosion time and corrosion depth was obtained when the diameter of the through hole at the bottom of the glass and the corrosion current remained unchanged. Figure 2 As shown, the corrosion depth can be precisely controlled by controlling the corrosion time. In this embodiment, the surface morphology and microscopic morphology of the corrosion pits are as follows: Figure 3-8 shown.
[0050] S5. Stress detection: XSTRESS DST-17 stress meter is used to measure each corrosion position. Mn target is used as X-ray target with wavelength of The residual stress of the composite plate was measured by the tilt method, with a starting angle of 150°, an end angle of 155°, a step width of 0.04°, and a test time of 0.3s for each step width. The DST-177 high-resolution X-ray stress tester had a tube voltage of 25kV and a tube current of 25mA. The measurement position and direction of the composite plate were kept consistent for each measurement, and two sets of data were measured at each position to take the average value. Then the process of steps S2-S5 was repeated until the corrosion depth reached the required depth and the stress detection was completed.
[0051] According to the depth measured each time and the stress value detected, draw a trend graph of the depth and stress distribution along the layer depth. Fig. 9 The figure shows the distribution of residual stresses on the surface, far interface, near interface and interface of the composite plate at different positions along the rolling direction.
[0052] Example 2
[0053] In this example, a composite plate with 304 stainless steel as the cladding material and Q235 as the substrate is rolled. After rolling, the residual stress distribution within the range of 1.5 mm from the surface position to the interface position on the 304 stainless steel side of the composite plate is measured using the method of the present invention. This example mainly studies the variation law of the residual stress on the 304 stainless steel side within the depth range, so the experimental steps are all carried out on the 304 stainless steel side. The specific operation steps are as follows:
[0054] S1. Surface treatment: First, clean the iron oxide on the side surface of the composite plate 304 stainless steel, then polish it with 1000-grit sandpaper, and then wipe the surface repeatedly with acetone until all the stains on the surface are cleaned.
[0055] S2. Paste the glass cup: Select the measurement position along the rolling direction and transverse direction of the metal composite plate, and take 2 special glass cups with an inner diameter of 30mm and a bottom through hole of 7mm. The through hole is set at the center of the bottom of the cup, 30mm high and 1mm thick. Then apply glue evenly on the bottom of the glass cup, paste the glass cups on the stainless steel surface respectively, and align the through hole with the measurement position. During this process, rotate the glass cup around the center to ensure that there is glue between the glass cup and the stainless steel without gaps. During this process, it should be ensured that the stainless steel surface at the through hole position is not stained with glue to avoid affecting the corrosion effect. Wait until the glue is dry and the glass cup is firmly attached to the stainless steel side.
[0056] S3, electrolytic corrosion: The electrolytic corrosion stripping method is selected. The device used for electrolytic corrosion stripping consists of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material. The specific operation is as follows: add two-thirds of the electrolyte to the glass cup attached to the metal composite plate. The electrolyte is a saturated NaCl solution, and then connect one end of the graphite rod to one end of the negative electrode, insert the other end of the graphite rod into the electrolyte in the glass cup 4-5mm, and connect the other end of the negative electrode to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the measured material, and the other end is connected to the positive electrode of the voltage-stabilized power supply through a wire. After checking the circuit path, start the power switch, adjust the current to stabilize at 2A, and then start timing.
[0057] S4. Corrosion depth measurement: Through experiments, we have obtained the corresponding relationship between corrosion time and corrosion depth while keeping the diameter of the through hole at the bottom of the glass cup and the corrosion current unchanged. By controlling the corrosion time, we can accurately control the corrosion depth. In this example, the corrosion was carried out for 25 minutes. The microscopic photos of the corrosion pits are shown in the figure below. Fig.10 shown.
[0058] S5. Stress detection: XSTRESS DST-17 stress meter is used to measure each corrosion position. Mn target is used as X-ray target with wavelength of The residual stress of the composite plate was measured by the tilt method, with a starting angle of 150°, an end angle of 155°, a step width of 0.04°, and a test time of 0.3s for each step width. The DST-177 high-resolution X-ray stress tester had a tube voltage of 25kV and a tube current of 25mA. The measurement position and direction of the composite plate were kept consistent for each measurement, and two sets of data were measured at each position to take the average value. Then the process of steps S2-S5 was repeated until the corrosion depth reached the required depth and the stress detection was completed.
[0059] Example 3
[0060] In this example, a composite plate with industrial pure titanium TA1 as the cladding material and 6061Al as the substrate is used. After rolling, the residual stress distribution of the 6061Al side of the composite plate within a depth range of 2 mm from the surface position to the interface position is measured using the method of the present invention. This example mainly studies the variation law of the residual stress on the 6061Al side within the depth range, so the experimental steps are all carried out on the 6061Al side. The specific operation steps are as follows:
[0061] S1. Surface treatment: First, grind the side surface of the composite board 6061Al with 1000-grit sandpaper, and then wipe the surface repeatedly with acetone until all stains on the surface are cleaned.
[0062] S2. Paste the glass cup: Select the measurement position along the rolling direction and transverse direction of the metal composite plate, and take 2 special glass cups with an inner diameter of 30mm and a bottom through hole diameter of 7mm. The through hole is set at the center of the bottom of the cup, 30mm high, and 1mm thick. Then apply glue evenly on the bottom of the glass cup, paste the glass cups on the surface of 6061Al respectively, and align the through hole with the measurement position. During this process, rotate the glass cup around the center to ensure that there is glue between the glass cup and 6061Al without gaps. During this process, it should be ensured that the surface of 6061Al at the through hole position is not stained with glue to avoid affecting the corrosion effect. Wait until the glue dries and the glass cup is firmly glued to the side of 6061Al.
[0063] S3, electrolytic corrosion: The electrolytic corrosion stripping method is selected. The device used for electrolytic corrosion stripping consists of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material. The specific operation is as follows: add two-thirds of the electrolyte to the glass cup attached to the metal composite plate. The electrolyte is a saturated NaCl solution, and then connect one end of the graphite rod to one end of the negative electrode, insert the other end of the graphite rod into the electrolyte in the glass cup 4-5mm, and connect the other end of the negative electrode to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the measured material, and the other end is connected to the positive electrode of the voltage-stabilized power supply through a wire. After checking the circuit path, start the power switch, adjust the current to stabilize at 2A, and then start timing.
[0064] S4. Corrosion depth measurement: Through experiments, we have obtained the corresponding relationship between corrosion time and corrosion depth while keeping the diameter of the through hole at the bottom of the glass cup and the corrosion current unchanged. By controlling the corrosion time, we can accurately control the corrosion depth. In this example, the corrosion was carried out for 40 minutes. The microscopic photos of the corrosion pits are shown in the figure below. Fig.11 shown.
[0065] S5. Stress detection: XSTRESS DST-17 stress meter is used to measure each corrosion position. Cr target is used as X-ray target with wavelength of The residual stress of the composite plate was measured by the tilt method, with a starting angle of 154°, an end angle of 160°, a step width of 0.04°, and a test time of 0.1s for each step width. The DST-177 high-resolution X-ray stress tester had a tube voltage of 25kV and a tube current of 40mA. The measurement position and direction of the composite plate were kept consistent for each measurement, and two sets of data were measured at each position to take the average value. Then the process of steps S2-S5 was repeated until the corrosion depth reached the required depth and the stress detection was completed.
[0066] The present invention is a method for measuring the residual stress of a composite plate material, and is particularly suitable for measuring the residual stress of a material in a depth direction. By actually operating the method in an embodiment, we obtain the distribution of residual stresses of the composite plate material at different positions along the rolling direction, at the surface, at the far interface, at the near interface and at the interface.
Claims
1. A method for measuring residual stress distributed locally along the layer depth of a metal composite plate, characterized in that: The steps include: S1. Surface treatment: Grind and clean the surface of the metal composite plate, and try to ensure that the measuring position is flat, and then wipe the surface clean with alcohol; S2. Paste the glass cup: Select the measurement position in a distributed manner along the rolling direction and transverse direction of the metal composite plate, and then paste one or more glass cups with through holes at the bottom to the measurement position. The through holes at the bottom of the glass cup should be tightly pasted to the metal composite plate without any gaps to ensure that the electrolyte will not leak from the gaps at the bottom of the cup during the corrosion process. The through holes at the bottom of the glass cup should be aligned with the measurement point, and then wait for the glue to dry; S3, electrolytic corrosion: the electrolytic corrosion stripping method is selected; the specific operation includes: the device used in the electrolytic corrosion stripping method is composed of a voltage-stabilized power supply, positive and negative electrodes, a glass cup, a graphite rod, and a test material; an electrolyte is added to a depth of two-thirds into the glass cup attached to the metal composite plate, and the electrolyte is a saturated NaCl solution, and then one end of the graphite rod is connected to one end of the negative electrode, and the other end of the graphite rod is inserted into the electrolyte in the glass cup, and the other end of the negative electrode is connected to the negative electrode of the voltage-stabilized power supply; one end of the positive electrode is directly connected to the test material, and the other end thereof is connected to the positive electrode of the voltage-stabilized power supply through a wire; the metal composite plate at the through hole at the bottom of the glass cup is locally electrolytically stripped layer by layer using a power supply device; S4. Corrosion depth measurement: Keep the corrosion current constant, change the corrosion time, measure the corrosion depth at different corrosion times, and obtain the variation law of the corrosion depth of the corroded material with the corrosion time; S5, stress detection: measure each corrosion position, and ensure that the measurement position and direction of the metal composite plate remain consistent during each measurement; then loop through steps S2 to S5 until the corrosion depth reaches the required depth and the stress detection is completed.
2. The method for measuring the residual stress distributed locally along the layer depth of a metal composite plate according to claim 1 is characterized in that: In the step S1, the surface treatment of the metal composite plate is carried out by ultrasonic cleaning, mechanical grinding and pickling to remove rust and oil stains on the surface, as well as high-pressure cleaning and drying.
3. The method for measuring the residual stress distributed locally along the layer depth of a metal composite plate according to claim 1, characterized in that: In step S2, the glass is a specially made glass with an inner diameter of 30-50 mm, a height of 30-50 mm, a wall thickness of 1-5 mm, a bottom through hole with a diameter of 4-12 mm, and the through hole is arranged at the center of the bottom of the glass.
4. The method for measuring the residual stress of a metal composite plate distributed locally along the layer depth according to claim 1, characterized in that: In step S2, the number of the glasses is less than or equal to 5.
5. The method for measuring the residual stress distributed locally along the layer depth of a metal composite plate according to claim 1, characterized in that: In the step S2, the sticking positions of the glass cups are designed in a distributed manner along the rolling direction and the transverse direction of the composite plate.
6. The method for measuring the residual stress distributed locally along the layer depth of a metal composite plate according to claim 1, characterized in that: In step S5, the parameters of the X-ray stress measuring instrument are as follows: the wavelength of the X-ray is determined according to the selected target material, the residual stress of the composite plate is measured by the tilt method, the measurement starting angle is 150-154°, the end angle is 155-160°, the measurement step width is 0.04°, and the test time for each step width is 0.1-0.3s; at this time, the DST-177 high-resolution X-ray stress measuring instrument sets the measuring tube voltage to 10-25kV and the tube current to 5-40mA. The parameters of the above X-ray stress measuring instrument can be appropriately adjusted according to different corroded metal materials.
7. The method for measuring the residual stress distributed locally along the layer depth of a metal composite plate according to claim 1, characterized in that: The method is capable of measuring the residual stress of the metal composite plate at various depths within a depth of 2 mm from the surface.
Citation Information
Patent Citations
Device and method for controlling residual stress on surface of metal microstructure
CN101722361A
Additive product residual stress testing method
CN111207869A
Method for testing residual stress of steel thin welding plate with narrow welding seam characteristic
CN113203509A
Method for measuring internal residual stress of thick-wall circular tube
CN111337174A
Residual stress testing device and method based on electrolytic drilling
CN111637996A