Tantalum capacitor and manufacturing method thereof
By adopting porous body structure and silver film design in tantalum capacitors, the existing tantalum capacitors have solved the problem of ESR and LC at high frequencies, which improves capacity and reduces losses, simplifies the process flow, and achieves a small volume Large capacity and high frequency response requirements.
Patent Information
- Application Number
- CN202211497646.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-25
AI Technical Summary
The existing tantalum capacitors have a large ESR and a large LC at high frequencies, and the preparation process is complex and costly, making it difficult to meet the needs of small volume, large capacity and high frequency response speed.
The porous tantalum capacitor structure is adopted, including tantalum anode, dielectric oxide film, MnO2 or PEDOT film and silver film. The silver film adheres to the pores, further adding a silver paste layer or graphite layer, replacing some PEDOT layer, and simplifying the process flow.
The capacity of tantalum capacitors is increased, ESR, loss and LC is reduced, the preparation process is simplified, and the cost is reduced.
Smart Images

Figure CN115985690B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a tantalum capacitor and a manufacturing method thereof. Background Art
[0002] In recent years, with the rapid development of the integrated circuit industry, global electronic products have become increasingly miniaturized, which has correspondingly increased the requirements for small size of passive devices. At the same time, the electrical performance of the devices is required to meet the needs of the equipment, which requires the study of small-volume and large-capacity tantalum capacitors. In addition, with the continuous increase in the operating frequency of electronic circuits, tantalum capacitors are required to have a higher frequency response speed, so it is necessary to further reduce the ESR (equivalent series resistance) of tantalum capacitors. In order to ensure the reliability of capacitors, it is necessary to develop tantalum capacitors with low LC (leakage current). This urgently requires the improvement of the performance of tantalum capacitors.
[0003] Using MnO 2 When used as the cathode of tantalum capacitor, due to MnO 2 The low conductivity of MnO makes the ESR (equivalent series resistance) of tantalum capacitors relatively large, thus limiting their use at higher frequencies. 2 Tantalum capacitors have a larger LC.
[0004] When PEDOT (conductive polymer 3,4-ethylenedioxythiophene) is used as the cathode of tantalum capacitors, the process control of polymer tantalum capacitors is complex, resulting in differences in the conductivity of the inner polymer and excessively high product ESR. In addition, in the design of high-specific capacitance products, the existing process has bottlenecks, the pores of the tantalum block cannot be effectively penetrated, and the coverage rate is not high, resulting in too low product capacity.
[0005] In addition, the production process of tantalum capacitor cathodes is complex and the cycle is too long. If an error occurs in any step, the entire product will be scrapped and the manufacturing cost is high.
[0006] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention
[0007] The main purpose of the present invention is to overcome the defects of the above-mentioned background technology and provide a tantalum capacitor and a manufacturing method thereof.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A tantalum capacitor, which includes a tantalum anode, a dielectric oxide film, and a MnO 2 Or a PEDOT film, and a silver film, wherein the tantalum capacitor is a porous body, and the silver film is attached to the pores of the tantalum capacitor.
[0010] Further:
[0011] It also includes a silver paste layer located outside the silver film, wherein the tantalum capacitor is a porous body, and the silver film is attached to the pores of the tantalum capacitor.
[0012] Also included is a graphite layer located between the silver film and the silver paste layer.
[0013] The invention also includes another MnO film located between the silver film and the graphite layer. 2 Or PEDOT film.
[0014] The MnO 2 Or the thickness of the PEDOT film is 50-150nm, the thickness of the silver film is 200-500nm, and the thickness of the silver film in the tantalum capacitor micropores accounts for 10%-60% of the diameter of the tantalum capacitor micropores.
[0015] The dielectric oxide film is Ta 2 O 5 membrane.
[0016] A method for manufacturing a tantalum capacitor, comprising: forming a porous tantalum anode, a dielectric oxide film and a MnO 2 or PEDOT thin film tantalum block, characterized in that it also includes: in MnO 2 or the step of forming a silver film on a PEDOT film; or 2 or the step of sequentially forming a silver film and a silver paste layer on the PEDOT film; or 2 or the step of sequentially forming a silver film, a graphite layer and a silver paste layer on the PEDOT film; or 2 or PEDOT film, then a silver film, another MnO 2 Or the steps of PEDOT film, graphite layer and silver paste layer.
[0017] Further:
[0018] The steps of forming the silver film include: reducing a solution of a silver compound to metallic silver through a chemical reaction, infiltrating the pores of the tantalum capacitor with the silver compound, reducing the silver through a silver mirror reaction, and causing the silver to adhere to the pores of the tantalum capacitor as a cathode of the tantalum capacitor.
[0019] The steps of forming the silver paste layer include:
[0020] Add ammonia solution dropwise to silver nitrate solution. Initially, the solution shows brown precipitation. Continue to add dropwise until the brown precipitation just disappears, and obtain silver ammonia solution.
[0021] Soaking the tantalum block in the silver-ammonia solution and subjecting the silver-ammonia solution to a constant temperature water bath;
[0022] Glucose solution is added to the silver ammonia solution. After the silver ammonia solution becomes turbid, the glucose solution is continued to be added dropwise to reduce the silver ions in the silver ammonia solution to silver. 2 Or a silver film is formed on a PEDOT film.
[0023] The MnO 2 Or the thickness of the PEDOT film is 50-150nm, the thickness of the silver film is 200-500nm, and the thickness of the silver film in the tantalum capacitor micropores accounts for 10%-60% of the diameter of the tantalum capacitor micropores.
[0024] The present invention has the following beneficial effects:
[0025] The present invention provides a porous tantalum capacitor, in which MnO 2 Or a silver film is formed outside the PEDOT film, so that the silver film is attached to the pores inside the tantalum capacitor, and silver also serves as the cathode of the tantalum capacitor. Through this structure, it is different from the simple use of MnO 2 Compared with tantalum capacitors using PEDOT thin films as cathodes, the present invention increases the capacity of tantalum capacitors and reduces the ESR, loss and LC of tantalum capacitors; compared with tantalum capacitors using only PEDOT thin films as cathodes, the present invention increases the capacity of tantalum capacitors and reduces the ESR, loss and LC of tantalum capacitors; in addition, since the silver film can replace part of the PEDOT cathode layer, the PEDOT cathode layer previously required a multi-step process with many steps, while the preparation of the silver film is relatively simple, which also reduces the multi-step process flow and saves preparation time. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 FIG. 1 is a schematic diagram of a layered structure of a tantalum capacitor according to an embodiment of the present invention.
[0027] Figure 2 The thickness of silver film is 50-150nmMnO 2 A graph showing the effect of ESR on tantalum capacitors with PEDOT or thin films.
[0028] Figure 3 This is a SEM / EDS image of the cut edge of the PEDOT sample of Example 1.
[0029] Figure 4 This is a SEM / EDS image of the middle part of the cross section of the PEDOT sample of Example 1.
[0030] Figure 5 FIG. 4 is a schematic diagram of a layered structure of a tantalum capacitor according to another embodiment of the present invention.
[0031] Figure 6 FIG. 4 is a schematic diagram of a layered structure of a tantalum capacitor according to another embodiment of the present invention. DETAILED DESCRIPTION
[0032] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention.
[0033] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element. In addition, connection can be used for fixing as well as for coupling or communication.
[0034] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0035] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0036] like Figure 1 As shown, an embodiment of the present invention provides a tantalum capacitor, which includes at least a tantalum anode 1, a dielectric oxide film 2, and a MnO 2 or PEDOT film 3, and silver film 4. The tantalum capacitor is a porous body ( Figure 1 It is only a schematic diagram, and its porous structure is not directly shown). The pores 101 of the tantalum capacitor (see Figure 3 ) is attached with the silver film. This structure can increase the capacity of the tantalum capacitor and reduce the ESR, loss and LC of the tantalum capacitor.
[0037] In a preferred embodiment, Figure 5 As shown, the silver film 4 may be covered with a graphite layer 5 and a silver paste layer 6 in sequence. After adding the graphite layer and the silver paste layer, the silver film can be prevented from being damaged in the subsequent process flow and during use. As another variation of this embodiment, only the silver paste layer may be added without adding the graphite layer. However, adding the graphite layer can improve reliability.
[0038] In a more preferred embodiment, Figure 6 As shown, the silver film 4 can be covered with another MnO 2 or PEDOT film 7, graphite layer 5 and silver paste layer 6. In this embodiment, MnO 2 Or the PEDOT film can at least effectively prevent the diffusion of silver, further improving the reliability of the product.
[0039] Preferably, MnO 2 Or the thickness of the PEDOT film is 50-150nm, the thickness of the silver film 4 is 200-500nm, and the thickness of the silver film in the tantalum capacitor micropore accounts for 10%-60% of the diameter of the tantalum capacitor micropore. Preferably, the dielectric oxide film 2 is Ta 2 O 5 membrane.
[0040] The present invention also provides a method for manufacturing a tantalum capacitor, comprising: forming a tantalum anode 1, a dielectric oxide film 2 and a MnO2 film as a cathode. 2 or PEDOT film 3, further comprising: 2 or the step of forming a silver film 4 on the PEDOT film 3 ( Figure 1 ). Alternatively, in the MnO 2 or the step of sequentially forming a silver film 4, a graphite layer 5 and a silver paste layer 6 on a PEDOT film 3 ( Figure 5 ); or, in the MnO 2 or PEDOT film 3 is sequentially formed with a silver film 4, a MnO 2 or the step of forming a PEDOT film 7, a graphite layer 5 and a silver paste layer 6 ( Figure 6 ).
[0041] Since the tantalum capacitor of the embodiment of the present invention has MnO as the cathode 2 Or a silver film is formed on the PEDOT film, and the silver film is attached to the pores of the porous tantalum capacitor. Silver also serves as the cathode of the tantalum capacitor. Through this structure, it is different from the simple use of MnO 2 Compared with tantalum capacitors using a PEDOT film as a cathode, the present invention increases the capacity of the tantalum capacitor and reduces the ESR, loss and LC of the tantalum capacitor; compared with tantalum capacitors using only a PEDOT film as a cathode, the present invention also increases the capacity of the tantalum capacitor and reduces the ESR, loss and LC of the tantalum capacitor; in addition, since the silver film can replace part of the PEDOT cathode layer, the PEDOT cathode layer previously required a multi-step process with many steps, while the preparation of the silver film is relatively simple, which also reduces the multi-step process flow and saves preparation time.
[0042] The specific embodiments of the present invention are further described below.
[0043] In a specific embodiment, the method for manufacturing a tantalum capacitor may include the following process:
[0044] 1. Formation and sintering of tantalum blocks → 2. Energy supply → 3. Coating with a certain thickness of MnO 2 or PEDOT → 4. Prepare the solution required for preparing silver ammonia solution → 5. Prepare silver ammonia solution → 6. Soak tantalum block → 7. Form a silver film inside the tantalum block → 8. Cover with a certain thickness of MnO 2 Or PEDOT→9. Prepare graphite layer and silver paste layer→10. Dry and test.
[0045] Among them, steps 4-7 are used to form a silver film. Since silver has good conductivity, it can be used to form a silver film at a certain thickness. 2 Or prepare a certain thickness silver film on the basis of PEDOT cathode instead of MnO 2 Or PEDOT film, through the chemical reaction of silver compound solution being reduced to metallic silver, the pores of tantalum capacitor are infiltrated with silver compound, and silver is reduced through silver mirror reaction (chemical reaction of silver compound solution being reduced to metallic silver), so that silver is attached to the pores of tantalum block as the cathode of tantalum capacitor. The reaction equation is:
[0046] AgNO 3 +3NH 3 ·H 2 O→Ag(NH 3 ) 2 OH+NH 4 NO 3 +2H 2 O
[0047] 2Ag(NH 3 ) 2 OH+R-CHO→2Ag↓+R-COONH 4 +3NH 3 ↑+H 2 O
[0048] The specific steps are as follows:
[0049] 1. Press tantalum metal powder into a fixed shape, and then subject the formed compact to high temperature treatment. At high temperature, the tantalum block forms a porous body with appropriate porosity.
[0050] 2. Through electrochemical reaction, a dielectric oxide film grows on the inner and outer surfaces of the sintered tantalum block, namely Ta 2 O 5 .
[0051] 3. Preparation of MnO 2Thin film: Immerse the porous tantalum anode block in a manganese nitrate solution, take it out and dry it at high temperature after it is completely soaked, so that the manganese nitrate decomposes to produce a conductive MnO2 film. Repeat the steps to prepare a multilayer thin film. Alternatively, prepare a PEDOT film: Prepare the PEDOT cathode by a two-step in-situ polymerization method, soak the energized tantalum block in a monomer EDOT and an oxidant solution, and then go through the cleaning and drying steps. Repeat this step to prepare a multilayer thin film.
[0052] 4. Prepare the required type of tantalum capacitor samples and respectively prepare appropriate concentrations of silver nitrate, ammonia solution, and glucose solution.
[0053] 5. Take an appropriate amount of silver nitrate solution and put it into a beaker. Use a dropper to slowly add ammonia water into the silver nitrate solution. Initially, the solution will show a brown precipitate. Continue to add until the brown precipitate just disappears. At this time, the solution is a silver ammonia solution.
[0054] 6. Place the beaker containing the silver ammonia solution into a constant temperature water bath, and then add the required type of MnO 2 Or PEDOT cathode tantalum block is immersed in a beaker.
[0055] 7. Add the glucose solution to the silver ammonia solution. The solution will become turbid instantly. After adding more, a bright silver layer can be clearly observed on the wall of the beaker. This indicates that the silver ions have been reduced to silver. Take out the tantalum block.
[0056] 8. Repeat the process of step 3 to prepare another layer of MnO 2 film.
[0057] 9. In order to prevent the cathode layer from being damaged in the subsequent process flow and to enable the cathode to form a good electrical connection with the external circuit, graphite layers and silver paste layers are successively formed on the cathode layer.
[0058] 10. Place the tantalum block in an oven for drying, and then test the capacity, ESR, loss, and LC of the tantalum block.
[0059] Among them, step 8 and step 9 are optional but not required.
[0060] Embodiment 1
[0061] like Figure 1 As shown, the tantalum capacitor structure of this embodiment has a tantalum anode, a Ta 2 O 5 、MnO 2 or PEDOT film, and silver film. The tantalum capacitor structure of the preferred embodiment has a tantalum anode, a Ta 2 O 5 , 50-150nm MnO 2Or PEDOT film, 200-500nm silver film, the thickness of the silver film in the tantalum capacitor micropores accounts for 10%-60% of the diameter of the tantalum capacitor micropores. Compared with conventional tantalum capacitors, the capacitance of this tantalum capacitor is slightly increased, and the ESR, loss and LC are reduced.
[0062] Preparation method:
[0063] The reagents used are 2% silver nitrate and ammonia water, and 10% glucose. Silver films of different thicknesses are prepared on MnO2 or PEDOT films of different thicknesses. MnO2 or PEDOT and the silver film are used as cathodes. The experimental samples prepared include tantalum capacitors with 50-150nm MnO2 or PEDOT films, tantalum capacitors with 150-300nm MnO2 or PEDOT films, and tantalum capacitors with 300-450nm MnO2 or PEDOT films. The tantalum capacitor structure of this embodiment is as follows: Figure 1 shown.
[0064] Test results:
[0065] In general, when MnO 2 Or when the PEDOT film thickness is 50-150nm and the silver film thickness is 200-500nm, the tantalum capacitor has the largest capacitance, and the smallest ESR, loss value and LC. Figure 2 The effect of silver film thickness on 50-150nmMnO 2 The influence of the ESR of tantalum capacitors with or PEDOT film, as the thickness of the silver film increases, the capacitance of the tantalum capacitor increases first and then tends to be stable, and the ESR, loss value and LC decrease first and then tend to be stable. Table 1 shows the electrical properties of the normal process sample and the sample after the silver mirror reaction. The capacitance of the sample with silver film is slightly increased, and the ESR, loss and LC are reduced. Figure 3 and Figure 4 The SEM / EDS images of the edge and middle of the cross section of the PEDOT sample (PEDOT thickness 50-150nm, silver film thickness 200-500nm) are shown in Figure 1. Figure 3 (a) shows the SEM of the edge of the PEDOT sample section, and (b) shows the distribution of silver at the edge of the tantalum capacitor. Figure 4 (a) shows the SEM of the middle part of the PEDOT sample cross section, and (b) shows the distribution of silver inside the tantalum capacitor. The results show that silver has entered the pores of the tantalum block and is distributed relatively evenly inside the tantalum block. The silver content at the edge of the sample cross section is greater than that in the middle part of the cross section.
[0066] Table 1
[0067]
[0068] Embodiment 2
[0069] like Figure 5 As shown, the tantalum capacitor structure of this embodiment has a tantalum anode, a Ta 2 O 5 , 50-150nm MnO 2 Or PEDOT film, 200-500nm silver film, graphite layer and silver paste layer, wherein the thickness of the silver film in the tantalum capacitor micropore accounts for 10%-60% of the diameter of the tantalum capacitor micropore. Compared with the conventional structure tantalum capacitor, the capacitance of the tantalum capacitor in this embodiment is slightly improved, and the ESR, loss and LC are reduced.
[0070] Preparation method:
[0071] Using the same reagent as in Example 1, in the 50-150nm MnO 2 A 200-500 nm silver film is prepared on a PEDOT film, and then a graphite layer and a silver paste layer are prepared on the silver film to obtain MnO 2 Or a tantalum capacitor with a PEDOT film thickness of 50-150nm, whose structure is as follows Figure 5 shown.
[0072] Test results:
[0073] The electrical performance of the product was tested and it was found that after the graphite layer and the silver paste layer were added in this embodiment, the capacitance value and LC of the tantalum capacitor were almost unchanged, and the ESR and loss value were slightly increased.
[0074] Compared with the first embodiment, the addition of the graphite layer and the silver paste layer can prevent the silver film from being damaged in the subsequent process flow and during use.
[0075] Embodiment 3
[0076] like Figure 6 As shown, the tantalum capacitor structure of this embodiment comprises a tantalum anode, a Ta 2 O 5 , 50-150nm MnO 2 Or PEDOT film, 200-500nm silver film, 50-150nm MnO 2 Or PEDOT film, graphite layer and silver paste layer, wherein the thickness of the silver film in the tantalum capacitor micropore accounts for 10%-60% of the diameter of the tantalum capacitor micropore. Compared with conventional tantalum capacitors, the capacitance of the tantalum capacitor in this embodiment is slightly improved, and the ESR, loss and LC are reduced.
[0077] Preparation method:
[0078] Using the same reagent as in Example 1, a 50-150 nm thick MnO 2 Or prepare a 200-500nm silver film on a PEDOT film, and then prepare a 50-150nm MnO2 or PEDOT film, and finally prepare a graphite layer and a silver paste layer to obtain a double 50-150nm thick MnO 2 Or PEDOT film tantalum capacitor, its structure is as follows Figure 6 shown.
[0079] Test results:
[0080] Compared with the second embodiment, this embodiment adds a layer of MnO 2 Or PEDOT film, the thickness of the silver film is reduced, and the electrical performance of the product is tested to find that the capacitance value of the tantalum capacitor in this embodiment is slightly reduced, the ESR and loss value are slightly increased, and the LC is reduced.
[0081] Since silver is more active, this embodiment adds MnO 2 Or PEDOT film can effectively prevent the diffusion of silver and improve the reliability of the product.
[0082] The background section of the present invention may contain background information about the problem or environment of the present invention, but does not necessarily describe the prior art. Therefore, the content included in the background section is not an admission by the applicant that the prior art is available.
[0083] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A tantalum capacitor, characterized in that: It includes a tantalum anode, a dielectric oxide film, a MnO2 or PEDOT film, and a silver film from the inside to the outside, wherein the tantalum capacitor is a porous body, and the silver film is attached to the pores of the tantalum capacitor; Also includes a silver paste layer located outside the silver film; Also included is a graphite layer located between the silver film and the silver paste layer; Also included is another MnO2 or PEDOT film located between the silver film and the graphite layer.
2. The tantalum capacitor according to claim 1, characterized in that: The thickness of the MnO2 or PEDOT film is 50-150nm, the thickness of the silver film is 200-500nm, and the thickness of the silver film in the micropores of the tantalum capacitor accounts for 10%-60% of the diameter of the micropores of the tantalum capacitor.
3. The tantalum capacitor according to claim 1, characterized in that: The dielectric oxide film is a Ta2O5 film.
4. A method for manufacturing a tantalum capacitor, comprising: The step of forming a tantalum block having a porous tantalum anode, a dielectric oxide film and a MnO2 or PEDOT film as a cathode is characterized in that it also includes: the step of sequentially forming a silver film, another MnO2 or PEDOT film, a graphite layer and a silver paste layer on the MnO2 or PEDOT film, and the silver film is attached to the pores of the tantalum capacitor.
5. The method for manufacturing a tantalum capacitor according to claim 4, characterized in that: The steps of forming the silver film include: reducing a solution of a silver compound to metallic silver through a chemical reaction, infiltrating the pores of the tantalum capacitor with the silver compound, reducing the silver through a silver mirror reaction, and causing the silver to adhere to the pores of the tantalum capacitor as a cathode of the tantalum capacitor.
6. The method for manufacturing a tantalum capacitor according to claim 5, characterized in that: The steps of forming the silver paste layer include: Add ammonia solution dropwise to silver nitrate solution. Initially, the solution shows brown precipitation. Continue to add dropwise until the brown precipitation just disappears, and obtain silver ammonia solution. Soaking the tantalum block in the silver-ammonia solution and subjecting the silver-ammonia solution to a constant temperature water bath; Glucose solution is added to the silver ammonia solution. After the silver ammonia solution becomes turbid, the glucose solution is continuously added dropwise to reduce the silver ions in the silver ammonia solution to silver, thereby forming a silver film on the MnO2 or PEDOT film.
7. The method for manufacturing a tantalum capacitor according to any one of claims 4 to 6, characterized in that: The thickness of the MnO2 or PEDOT film is 50-150nm, the thickness of the silver film is 200-500nm, and the thickness of the silver film in the micropores of the tantalum capacitor accounts for 10%-60% of the diameter of the micropores of the tantalum capacitor.