A two-dimensional silicon-carbon composite material and its preparation method and application

The preparation of two-dimensional silicon-carbon composite material by ultra-speed freeze-drying method of nano-silicon and carbon source aqueous solution was solved, and the problem of insufficient conductivity and stability of silicon-based anode materials was achieved, and the excellent electrochemical performance and high efficiency of the anode materials of lithium-ion batteries were achieved. electrochemical properties.

CN115986078BActive Publication Date: 2024-12-03合肥国轩新材料科技有限公司
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211704713.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-12-03
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing silicon-based anode materials have insufficient conductivity and stability in lithium-ion batteries, and the preparation process of two-dimensional carbon materials such as graphene is complex and expensive, making it difficult to effectively improve electrochemical performance.

Method used

The two-dimensional silicon carbon composite material is prepared by extremely fast freeze-drying method of nano-silicon and carbon source aqueous solution. Si@C particles are formed through carbonization and pickling treatment, forming a layered structure and core-shell structure to increase the specific surface area and pore volume. Promote ion/electron transfer.

Benefits of technology

The excellent electrochemical performance of the negative electrode material of lithium-ion battery was achieved, significantly improved the reversible capacity and Coulomb efficiency, and maintained high capacity and high efficiency in multiple cycle tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115986078B_ABST
    Figure CN115986078B_ABST
Patent Text Reader

Abstract

The present invention discloses a two-dimensional silicon-carbon composite material, which is layered and composed of a plurality of Si@C layers arranged in a layered state, and Si@C particles are evenly distributed to form a Si@C layer. The present invention also discloses a method for preparing the above-mentioned two-dimensional silicon-carbon composite material, comprising the following steps: mixing nano-silicon with a carbon source aqueous solution, then freezing the solid at a very high speed, freeze-drying the solid, then carbonizing, and acid-washing to obtain the two-dimensional silicon-carbon composite material. The present invention also discloses the application of the above-mentioned two-dimensional silicon-carbon composite material in anode materials. The present invention also discloses a cathode material. The two-dimensional silicon-carbon composite material of the present invention has a large specific surface area and pore volume, and its layered structure and the core-shell structure of the Si@C particles are coupled, which can effectively alleviate the volume expansion of silicon during charging and discharging, and the highly conductive carbon shell can also promote the rapid transfer of ions / electrons; when the present invention is used as a cathode material for a battery, it exhibits excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon negative electrode materials, and in particular to a two-dimensional silicon-carbon composite material and a preparation method and application thereof. Background Art

[0002] Silicon / carbon composites can be obtained by combining silicon with carbonaceous materials in a variety of ways. Many disadvantages of silicon-based materials can be complemented by combining with carbon matrices. Carbon materials have high electrical conductivity, which effectively enhances the electron transfer ability of silicon-based materials. By taking advantage of the wide source of carbon materials and strong structural plasticity, silicon-carbon composites with different structures can be designed to improve structural stability and safety.

[0003] The carbon sources used include amorphous carbon, graphite, carbon nanotubes, carbon nanosheets, carbon fibers, carbon quantum dots, etc. The combination of silicon and carbon materials can effectively improve the conductivity and stability of silicon negative electrodes. Two-dimensional carbon materials have shown great advantages in improving the silicon-based negative electrodes of lithium-ion batteries. Two-dimensional carbon materials are represented by graphene. Because graphene has excellent electronic conductivity and high mechanical properties, it can accommodate the stress caused by large volume expansion and improve the electrochemical properties of composite materials. However, graphene or reduced graphene requires multiple steps to be produced, and its preparation process is complicated and expensive. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a two-dimensional silicon-carbon composite material and a preparation method and application thereof. The two-dimensional silicon-carbon composite material of the present invention has a large specific surface area and pore volume, and its layered structure and the core-shell structure of the Si@C particles are coupled, which can effectively alleviate the volume expansion of silicon during the charging and discharging process. The highly conductive carbon shell can also promote the rapid transfer of ions / electrons. When the present invention is used as a battery negative electrode material, it exhibits excellent electrochemical properties.

[0005] The present invention provides a two-dimensional silicon-carbon composite material. The two-dimensional silicon-carbon composite material is in a layered state, composed of a plurality of Si@C layers arranged in a layered state, and Si@C particles are evenly distributed to form a Si@C layer.

[0006] The specific surface area of ​​the above two-dimensional silicon-carbon composite material is 265-280m 2 / g.

[0007] The pore volume of the two-dimensional silicon-carbon composite material is 0.299-0.337 cm 3 / g.

[0008] The present invention also discloses a method for preparing the above-mentioned two-dimensional silicon-carbon composite material, comprising the following steps: mixing nano-silicon with a carbon source aqueous solution, then rapidly freezing the mixture into a solid, freeze-drying the solid, then carbonizing it, and acid-washing it to obtain the two-dimensional silicon-carbon composite material.

[0009] Preferably, the carbon source is sulfonated naphthalene. Sulfonated naphthalene refers to a compound containing a naphthalene ring with a sulfonate group grafted onto the naphthalene ring. The sulfonated naphthalene selected in the present invention may be β-naphthalenesulfonic acid or the like.

[0010] Preferably, the mass ratio of nano-silicon to carbon source is 0.5-2:1.

[0011] Preferably, it is flash frozen in liquid nitrogen.

[0012] Preferably, the freeze-drying temperature is -20°C to -5°C, and the freeze-drying time is 40-60 hours.

[0013] Preferably, the carbonization is carried out in an inert gas atmosphere; the carbonization temperature is 850° C.-950° C., and the carbonization time is 1.5-2.5 h.

[0014] Preferably, hydrochloric acid is used for pickling, and the pickling time is 20-28 hours.

[0015] The nano-silicon and the carbon source aqueous solution are ultrasonically stirred for 1-2 hours to mix evenly; preferably, the stirring speed is 2000-3000 rpm.

[0016] After the above-mentioned rapid freezing into a solid, freeze-drying treatment is quickly performed.

[0017] After the above acid washing, the two-dimensional silicon-carbon composite material is obtained by washing with water and drying.

[0018] The present invention also proposes the application of the above two-dimensional silicon-carbon composite material in negative electrode materials.

[0019] The present invention also proposes a negative electrode material, the raw materials of which include, by weight: 7.5-8.5 parts of the above-mentioned two-dimensional silicon-carbon composite material, 0.75-1.25 parts of a conductive agent, and 0.75-1.25 parts of a binder.

[0020] The conductive agent may be conductive carbon black or the like, and the binder may be polyvinylidene fluoride, sodium alginate or the like.

[0021] Beneficial effects:

[0022] Reference Figure 1 The present invention utilizes an ice template method to mix nano-silicon and a carbon source aqueous solution, and then rapidly freezes the nano-silicon and the carbon source to obtain a solid distributed along the interface of the solvent crystals, and then rapidly freezes the solid to remove the solvent crystals, thereby obtaining a porous layered solid, and then carbonizes the nano-silicon surface (i.e., Si@C particles) to obtain a layered two-dimensional silicon-carbon composite material, wherein the Si@C particles are uniformly distributed to form a Si@C layer, and a plurality of Si@C layers are arranged to form a layered structure;

[0023] The two-dimensional silicon-carbon composite material of the present invention has a large specific surface area and pore volume, and the layered structure of the two-dimensional silicon-carbon composite material and the core-shell structure of the Si@C particles are coupled, which can effectively alleviate the volume expansion of silicon during the charge and discharge process, and the highly conductive carbon shell can also promote the rapid transfer of ions / electrons;

[0024] When the present invention is used as a negative electrode material for a lithium ion battery, it exhibits excellent electrochemical properties; the reversible capacity at a current density of 0.2 A / g can reach up to 2091 mAh / g, the first coulombic efficiency can reach up to 84.4%, after 300 cycles at a current density of 0.2 A / g, the capacity retention rate exceeds 95%, the coulombic efficiency can reach up to 99.86%, and the electrode material still maintains a reversible specific capacity of up to 374 mAh / g at a high rate of 5 A / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Diagram of the preparation mechanism of two-dimensional silicon-carbon composite materials. DETAILED DESCRIPTION

[0026] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0027] Example 1

[0028] A method for preparing a two-dimensional silicon-carbon composite material comprises the following steps:

[0029] Add nano-silicon particles to a mixture of ethanol and acetone in a volume ratio of 1:1, stir for 2 hours, centrifuge for 30 minutes, put the nano-silicon into a vacuum drying oven, keep it at 80°C for 12 hours, and set aside;

[0030] Weigh 0.5 g of β-naphthalenesulfonic acid and dissolve it in 200 ml of deionized water. After magnetic stirring for 30 min, filter it with a 0.22 μm microporous membrane to obtain a carbon source aqueous solution; take 1 g of the reserved nano-silicon and add it to the carbon source aqueous solution, and stir it at a speed of 2000 rpm in an ultrasonic cleaning machine for 2 h to evenly disperse the nano-silicon in the carbon source aqueous solution;

[0031] The solid is then quickly frozen in liquid nitrogen and quickly placed in a freeze dryer for continuous freeze drying at -20°C for 40 hours. The freeze-dried solid is then placed in a tubular furnace filled with argon and carbonized at 950°C for 1.5 hours. The carbonized material is then pickled with a hydrochloric acid solution for 20 hours, and then washed with water and dried to obtain a two-dimensional silicon-carbon composite material.

[0032] Example 2

[0033] A method for preparing a two-dimensional silicon-carbon composite material comprises the following steps:

[0034] Add nano-silicon particles to a mixture of ethanol and acetone in a volume ratio of 1:1, stir for 2 hours, centrifuge for 30 minutes, put the nano-silicon into a vacuum drying oven, keep it at 80°C for 12 hours, and set aside;

[0035] Weigh 0.5 g of β-naphthalenesulfonic acid and dissolve it in 200 ml of deionized water. After magnetic stirring for 30 min, filter it with a 0.22 μm microporous membrane to obtain a carbon source aqueous solution; take 1 g of the reserved nano-silicon and add it to the carbon source aqueous solution, and stir it at a high speed of 3000 rpm in an ultrasonic cleaning machine for 1 h to evenly disperse the nano-silicon in the carbon source aqueous solution;

[0036] The solid is then quickly frozen in liquid nitrogen and quickly placed in a freeze dryer for continuous freeze drying at -10°C for 60 hours. The freeze-dried solid is then placed in a tubular furnace filled with argon and carbonized at 850°C for 2.5 hours. The carbonized material is then pickled with hydrochloric acid solution for 28 hours, and then washed with water and dried to obtain a two-dimensional silicon-carbon composite material.

[0037] Example 3

[0038] A method for preparing a two-dimensional silicon-carbon composite material comprises the following steps:

[0039] Add nano-silicon particles to a mixture of ethanol and acetone in a volume ratio of 1:1, stir for 2 hours, centrifuge for 30 minutes, put the nano-silicon into a vacuum drying oven, keep it at 80°C for 12 hours, and set aside;

[0040] Weigh 0.5 g of β-naphthalenesulfonic acid and dissolve it in 200 ml of deionized water. After magnetic stirring for 30 min, filter it with a 0.22 μm microporous membrane to obtain a carbon source aqueous solution; take 1 g of the reserved nano-silicon and add it to the carbon source aqueous solution. In an ultrasonic cleaning machine, stir it at a speed of 2400 rpm for 1 h to evenly disperse the nano-silicon in the carbon source aqueous solution;

[0041] The solid is then quickly frozen in liquid nitrogen and placed in a freeze dryer for continuous freeze drying at -10°C for 48 hours. The freeze-dried solid is then placed in a tubular furnace filled with argon and carbonized at 900°C for 2 hours. The carbonized material is then pickled with hydrochloric acid solution for 24 hours, and then washed with water and dried to obtain a two-dimensional silicon-carbon composite material.

[0042] Example 4

[0043] The amount of β-naphthalenesulfonic acid is 1 g, and the other steps are the same as those in Example 3.

[0044] Example 5

[0045] The amount of β-naphthalenesulfonic acid is 2 g, and the other steps are the same as those in Example 3.

[0046] The specific surface area and pore volume of the two-dimensional silicon-carbon composite materials prepared in Examples 1-5 were tested, and the results are shown in Table 1.

[0047] Table 1 Test results

[0048] Test items Example 1 Example 2 Example 3 Example 4 Example 5 <![CDATA[Specific surface area m 2 / g]]> 274 280 265 278 267 <![CDATA[Pore volume cm 3 / g]]> 0.299 0.337 0.305 0.325 0.318

[0049] It can be seen from Table 1 that the two-dimensional silicon-carbon composite material prepared in the present invention has a large specific surface area and pore volume.

[0050] Comparative Example 1: Commercially available Si@C particles.

[0051] The two-dimensional silicon-carbon composite materials prepared in Examples 1-5 and Comparative Example 1 were taken as samples to prepare electrode sheets respectively, and the specific steps were as follows:

[0052] The sample, conductive carbon black, and binder polyvinylidene fluoride were ground in an agate mortar at a mass ratio of 8:1:1 for 1 h, then transferred to a glass cup, and appropriate amounts of N-methyl-2-pyrrolidone and deionized water were added, and magnetic stirring was performed for 24 h to form a slurry with uniform dispersion and moderate viscosity;

[0053] Take a copper current collector with a thickness of 0.12 mm, polish it with sandpaper and attach it to a flat glass plate, rinse the surface with alcohol to completely attach the copper current collector to the surface of the glass plate, then transfer the slurry and evenly coat it on the surface of the copper current collector, then put it into a vacuum drying oven and dry it at 90°C for 10 h to obtain an electrode sheet, and use a manual slicer MSK-110 to punch the completely dried electrode sheet into a circular electrode sheet with a diameter of 14 mm, weigh and record it, and then keep it in the glove box for later use.

[0054] The above circular electrode sheets are used to assemble CR2016 button-type half-cells, and the specific steps are as follows:

[0055] The metal lithium sheet is used as the counter electrode, and the circular electrode sheet is used as the negative electrode; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent of the electrolyte is a mixed solution of EC+DMC with a volume ratio of 1:1, and contains 5 wt% of fluoroethylene carbonate;

[0056] In a vacuum glove box filled with argon, the negative electrode shell, metal lithium sheet, Celgard2400 polypropylene diaphragm, negative electrode sheet, gasket, and positive electrode shell were assembled in the order of the negative electrode shell. During the whole process, the water and oxygen content in the glove box were less than 0.1ppm. After the half-cell was assembled, it was placed for 12 hours and then electrochemically tested. The results are shown in Table 2.

[0057] Table 2 Test results

[0058]

[0059]

[0060] It can be seen from Table 2 that the two-dimensional silicon-carbon composite material of the present invention has excellent electrochemical performance when used as a negative electrode material for lithium-ion batteries, which is much better than that of Comparative Example 1.

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A two-dimensional silicon-carbon composite material, characterized in that: The two-dimensional silicon-carbon composite material is layered, consisting of multiple Si@C layers arranged in layers, and Si@C particles are evenly distributed to form Si@C layers; The preparation method of the two-dimensional silicon-carbon composite material comprises the following steps: mixing nano-silicon with a carbon source aqueous solution, then rapidly freezing the solid, freeze-drying the solid, then carbonizing, and acid-washing to obtain the two-dimensional silicon-carbon composite material; The carbon source was sulfonated naphthalene; it was rapidly frozen in liquid nitrogen.

2. A method for preparing the two-dimensional silicon-carbon composite material as claimed in claim 1, characterized in that: The method comprises the following steps: mixing nano silicon and a carbon source aqueous solution, then rapidly freezing the solution into a solid, freeze-drying the solid, then carbonizing the solid, and acid washing the solid to obtain a two-dimensional silicon-carbon composite material.

3. The method for preparing the two-dimensional silicon-carbon composite material according to claim 2, characterized in that: The mass ratio of nano silicon to carbon source is 0.5-2:

1.

4. The method for preparing the two-dimensional silicon-carbon composite material according to claim 2 or 3, characterized in that: The freeze-drying temperature is -20°C to -5°C, and the freeze-drying time is 40-60h.

5. The method for preparing the two-dimensional silicon-carbon composite material according to claim 2 or 3, characterized in that: Carbonization is carried out in an inert gas atmosphere; the carbonization temperature is 850°C-950°C, and the carbonization time is 1.5-2.5h.

6. The method for preparing the two-dimensional silicon-carbon composite material according to claim 2 or 3, characterized in that: Use hydrochloric acid for pickling, and the pickling time is 20-28h.

7. An application of the two-dimensional silicon-carbon composite material as claimed in claim 1 in negative electrode materials.

8. A negative electrode material, characterized in that The raw materials include, by weight: 7.5-8.5 parts of the two-dimensional silicon-carbon composite material as claimed in claim 1, 0.75-1.25 parts of a conductive agent, and 0.75-1.25 parts of a binder.

Citation Information

Patent Citations

  • Preparation method for negative electrode material with core-shell coated structure and for lithium ion battery

    CN106941164A

  • Preparation method of porosity controllable graphene modified silicon-carbon composite material

    CN109873136A

  • Two-dimensional silicon nanosheet self-assembled silicon-carbon microsphere composite material, preparation method thereof and application of silicon-carbon microsphere composite material in negative electrode material of lithium ion battery

    CN111952559A

  • Preparation method of transition metal-N-C material with two-dimensional nanosheet structure and application of transition metal-N-C material to lithium-sulfur battery

    CN112007680A

  • Preparation method and application of carbon fiber / silicon carbide oriented porous skeleton

    CN113754454A