Modified diaphragm, solid electrolyte based on modified diaphragm and preparation method thereof

Through the solid-liquid method, nano-oxides are uniformly dispersed in the separator and combined with polymer solid electrolyte membrane, the problem of insufficient dispersion of nano-oxides in the prior art is solved, the migration number and mechanical properties of solid electrolytes are improved, and the battery is reduced Short circuit risk, extends battery life and enhances safety.

CN115986309BActive Publication Date: 2024-11-05HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310053405.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-03
Publication Date
2024-11-05
Estimated Expiration
2043-02-03

AI Technical Summary

Technical Problem

The dispersion of nano-oxides in existing separators is insufficient, which affects the mechanical strength and heat resistance of the solid electrolytes, and has a high electronic conductivity, resulting in an increase in the risk of battery short-circuiting, making it difficult to meet the requirements of lithium ion migration number and electrochemical stability window.

Method used

The solid-liquid method is used to immerse the hydroxyl-rich separator in an organic solvent and react with liquid metal halides to generate uniformly dispersed nanooxides. The modified separator is constructed in combination with the polymer solid electrolyte membrane to improve the number of lithium ion migration and mechanical properties. .

Benefits of technology

The uniform dispersion of nanooxides on the separator is achieved, the number of migration and mechanical properties of solid electrolytes are improved, the electronic conductivity is reduced, the battery life is extended and the safety is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115986309B_ABST
    Figure CN115986309B_ABST
Patent Text Reader

Abstract

The invention discloses a modified diaphragm, a solid electrolyte based on the modified diaphragm and a preparation method thereof, and belongs to the technical field of solid electrolyte preparation. The preparation method of the modified diaphragm is prepared according to the following steps: a diaphragm rich in hydroxyl is immersed in an organic solvent A, a liquid metal halide is added, and at room temperature, the hydroxyl and the halogen element react to generate a metal oxide to obtain a modified diaphragm. The method makes the nano oxide evenly dispersed on the diaphragm. A polymer and a lithium salt are dissolved in an organic solvent B, stirred evenly and then coated on the modified diaphragm, so as to obtain a solid electrolyte based on the modified diaphragm with a high migration number and good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolyte preparation, and more specifically to a modified diaphragm, a solid electrolyte based on the modified diaphragm and a preparation method thereof. Background Art

[0002] Replacing liquid electrolytes with solid electrolytes is an effective optimization strategy for applying lithium metal to energy storage. As a medium for transmitting lithium ions, solid electrolytes require high lithium ion conductivity; as a separator between positive and negative electrode materials, they need to have low electronic conductivity to prevent internal short circuits in the battery. Usually, the electronic conductivity of the material is required to be less than 10 -5 ~10 -3 S / cm; it must have a large lithium ion migration number and be as close to 1 as possible to reduce concentration polarization during the charge and discharge process and support high current charge and discharge; it must have a wide electrochemical stability window and undergo redox reactions during battery operation to extend the battery cycle life; it must have good interface contact with the electrode material and not react chemically with the electrode material or the current collector, have good chemical stability, and not be easy to decompose, burn or explode; it must have good mechanical properties, be able to resist external forces during the processing and application of the battery, be able to prevent the puncture of lithium dendrites, and improve the battery safety factor; it must have good heat dissipation performance and reduce the cost of battery thermal management and other performance requirements.

[0003] Diaphragm-modified solid electrolyte is a type of solid electrolyte, mainly composed of a diaphragm (polyethylene, polypropylene, cellulose, etc.) and a polymer solid electrolyte (polyethylene oxide, polyvinylidene fluoride, polymethyl methacrylate, etc.). Most of the existing commercial diaphragms use a polypropylene (PP) diaphragm coated with nano-alumina, and then a polyethylene oxide solid electrolyte is coated on this basis. This diaphragm-modified solid electrolyte can effectively improve the mechanical strength and heat resistance of the electrolyte, thereby extending the service life of the membrane. However, the coated nano-oxides mostly exist on the surface of the diaphragm, and their dispersibility on the surface also needs to be improved. Summary of the invention

[0004] In view of the above problems, the present invention provides a modified diaphragm, a solid electrolyte based on the modified diaphragm and a preparation method thereof, so that nano-oxides are uniformly dispersed on the diaphragm.

[0005] The first object of the present invention is to provide a method for preparing a modified diaphragm, which is prepared according to the following steps:

[0006] The hydroxyl-rich membrane is immersed in an organic solvent A, and liquid metal halide is added. At room temperature, the hydroxyl and halogen elements react to generate metal oxides to obtain a modified membrane.

[0007] Preferably, the volume ratio of organic solvent A to liquid metal halide is 5-200:1, and the reaction time is 4-24 hours.

[0008] Preferably, the hydroxyl-rich membrane is a cellulose porous membrane, a hydroxyl-modified polyethylene membrane or a hydroxyl-modified polypropylene membrane.

[0009] Preferably, the organic solvent A is one of n-hexane, toluene, carbon dichloride and p-xylene.

[0010] Preferably, the liquid metal halide includes, but is not limited to, titanium tetrachloride, boron trichloride, vanadium tetrachloride, and tin tetrachloride.

[0011] The second object of the present invention is to provide a modified diaphragm prepared by the above preparation method.

[0012] The third object of the present invention is to provide a solid electrolyte based on the modified diaphragm, comprising a modified diaphragm and a polymer solid electrolyte membrane, wherein the thickness ratio of the polymer solid electrolyte membrane to the modified diaphragm is (1:10) to (10:1); the coating density of the polymer solid electrolyte membrane is 50-99%;

[0013] The polymer solid electrolyte membrane is composed of a polymer substrate and a lithium salt, wherein the lithium salt accounts for 20% to 80% of the mass of the polymer substrate;

[0014] The solid electrolyte based on the modified separator was prepared according to the following steps:

[0015] The polymer substrate and lithium salt are dissolved in an organic solvent B, stirred evenly and then coated on the modified diaphragm, and vacuum dried to obtain a solid electrolyte based on the modified diaphragm.

[0016] Preferably, the polymer substrate is selected from one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide-polypropylene oxide-polyethylene oxide, polymethyl methacrylate, polyacrylonitrile, and polyvinyl chloride.

[0017] Preferably, the lithium salt is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)amide, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate and lithium dioxalatoborate.

[0018] Preferably, the organic solvent B is one of tetrahydrofuran, acetonitrile, N,N-dimethylformamide, N-methylpyrrolidone and acetone.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention is based on a solid-liquid method to prepare a nano-oxide dispersed diaphragm. The method is characterized in that a solid-liquid reaction is used to react hydroxyl groups and halogen elements, and the obtained nano-oxides are not only uniformly dispersed on the surface of the diaphragm, but also uniformly dispersed in the inner layer of the diaphragm, thereby truly achieving the purpose of uniformly dispersing the nano-oxides on the diaphragm.

[0021] The solid electrolyte based on the modified diaphragm is based on the modified diaphragm as the substrate, and then the substrate is coated with a polymer solid electrolyte membrane to construct a solid electrolyte membrane. The method is expected to use a simple solid-liquid method to obtain a modified diaphragm substrate uniformly dispersed on the diaphragm, and to construct a solid electrolyte membrane on this substrate. The obtained solid electrolyte membrane has a high migration number and good mechanical properties. This method has the advantages of simple design and controllable product structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanned image of the modified cellulose membrane prepared in Example 2;

[0023] Figure 2 IT curve of a solid electrolyte membrane composed of a cellulose membrane modified with a PVDF polymer and nano-boron oxide particles prepared in Example 2;

[0024] Figure 3 is a scanned image of the unmodified cellulose separator in Comparative Example 1;

[0025] Figure 4 IT curve of the solid electrolyte membrane composed of PVDF polymer and unmodified cellulose membrane prepared in Comparative Example 1. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] The liquid metal halide used in this embodiment is titanium tetrachloride solution (TiCl4, 2mL); the polymer substrate is polyethylene oxide (PEO), and the lithium salt is lithium bis(trifluoromethylsulfonyl)amide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI). The mass ratio of LiTFSI to LiFSI is 1:1, and the mass of the lithium salt is 50% of the mass of PEO; the polymer solid electrolyte membrane is 1 / 2 of the thickness of the modified diaphragm; the coating density of the polymer solid electrolyte membrane is 75%. The cellulose porous diaphragm used in this embodiment has a thickness of 45μm and a porosity of 38%.

[0029] The specific steps are as follows:

[0030] (1) Dry the cellulose porous membrane in a vacuum oven at 80° C. for 24 h, and then completely immerse the membrane in 20 mL of n-hexane solvent;

[0031] (2) Add 2 mL of titanium tetrachloride solution to the above n-hexane solvent and react at 25° C. for 4 h;

[0032] (3) taking out the cellulose membrane and drying it in a vacuum oven at 80° C. for 24 h to obtain a modified cellulose membrane with good TiO2 dispersion;

[0033] (4) 1 g PEO and 0.5 g lithium salt (LiTFSI, LiFSI) were mixed evenly, 20 mL acetone was added, and mechanical stirring was carried out at 25 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0034] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper, and vacuum dried in an oven at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0035] Example 2

[0036] The liquid metal halide used in this embodiment is a boron trichloride solution (BCl3, 0.5mL); the polymer substrate is polyvinylidene fluoride (PVDF), the lithium salt is lithium bis(oxalatoborate) (LiBOB), and the mass of the lithium salt is 50% of the mass of PVDF; the polymer solid electrolyte membrane is 1 / 2 of the thickness of the modified diaphragm; the coating density of the polymer solid electrolyte membrane is 75%. The cellulose porous diaphragm used in this embodiment has a thickness of 45μm and a porosity of 38%.

[0037] The specific steps are as follows:

[0038] (1) Dry the cellulose porous membrane in a vacuum oven at 60° C. for 24 h, and then completely immerse the membrane in 20 mL of p-xylene solvent;

[0039] (2) Add 0.5 mL of boron trichloride solution to the above-mentioned p-xylene solvent and react at 25° C. for 8 h;

[0040] (3) taking out the cellulose membrane and drying it in a vacuum oven at 60° C. for 24 h to obtain a modified cellulose membrane with good boron oxide dispersion;

[0041] (4) 1 g PVDF and 0.5 g lithium salt (LiBOB) were mixed evenly, 20 mL tetrahydrofuran was added, and mechanical stirring was performed at 25 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0042] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper, and vacuum dried in an oven at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0043] Example 3

[0044] The liquid metal halide used in this embodiment is vanadium tetrachloride solution (VCl4, 4mL); the polymer substrate is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and the lithium salt is lithium hexafluorophosphate (LiPF6), and the mass of the lithium salt is 20% of the mass of PVDF-HFP; the polymer solid electrolyte membrane is 1 / 10 of the thickness of the modified diaphragm; the coating density of the polymer solid electrolyte membrane is 50%. The cellulose porous diaphragm used in this embodiment has a thickness of 45μm and a porosity of 38%.

[0045] The specific steps are as follows:

[0046] (1) Dry the porous cellulose membrane in a vacuum oven at 60° C. for 24 h, and then completely immerse the membrane in 20 mL of carbon dichloride solvent;

[0047] (2) Add 4 mL of vanadium tetrachloride solution dropwise to the above carbon dichloride solvent and react at 25° C. for 10 h;

[0048] (3) taking out the cellulose membrane and drying it in a vacuum oven at 60° C. for 24 h to obtain a modified cellulose membrane with good dispersion of vanadium oxide;

[0049] (4) 1 g PVDF-HFP and 0.2 g lithium salt (LiPF6) were mixed evenly, 20 mL N-methylpyrrolidone (NMP) was added, and mechanical stirring was performed at 60 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0050] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper and dried at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0051] Example 4

[0052] The liquid metal halide used in this embodiment is tin tetrachloride solution (SnCl4, 0.1mL); the polymer substrate is polyethylene oxide-polypropylene oxide-polyethylene oxide (P123), and the lithium salt is lithium tetrafluoroborate (LiBF4), and the mass of the lithium salt is 80% of the mass of P123; the thickness of the polymer solid electrolyte membrane and the thickness of the modified diaphragm are 1:1; the coating density of the polymer solid electrolyte membrane is 99%. The thickness of the cellulose porous diaphragm used in this embodiment is 45μm, and the porosity is 38%.

[0053] The specific steps are as follows:

[0054] (1) Dry the cellulose porous membrane in a vacuum oven at 60° C. for 24 h, and then completely immerse the membrane in 20 mL of toluene solvent;

[0055] (2) Add 0.1 mL of vanadium tetrachloride solution dropwise to the toluene solvent and react at 25° C. for 24 h;

[0056] (3) taking out the cellulose membrane and drying it in a vacuum oven at 60° C. for 24 h to obtain a modified cellulose membrane with good dispersion of vanadium oxide;

[0057] (4) 1 g P123 and 0.8 g lithium salt (LiBF4) were mixed evenly, 20 mL N, N-dimethylamide was added, and mechanical stirring was carried out on a heating table at 60 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0058] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper and dried at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0059] Example 5

[0060] The liquid metal halide used in this embodiment is tin tetrachloride solution (SnCl4, 0.1mL); the polymer substrate is polymethyl methacrylate (PMMA), the lithium salt is lithium difluorooxalate borate (LiDFOB), and the mass of the lithium salt is 60% of the mass of PMMA; the thickness ratio of the polymer solid electrolyte membrane to the modified diaphragm is 1:5; the coating density of the polymer solid electrolyte membrane is 80%. The cellulose porous diaphragm used in this embodiment has a thickness of 45μm and a porosity of 38%.

[0061] The specific steps are as follows:

[0062] (1) Dry the cellulose porous membrane in a vacuum oven at 60° C. for 24 h, and then completely immerse the membrane in 20 mL of toluene solvent;

[0063] (2) Add 0.1 mL of vanadium tetrachloride solution dropwise to the toluene solvent and react at 25° C. for 24 h;

[0064] (3) taking out the cellulose membrane and drying it in a vacuum oven at 60° C. for 24 h to obtain a modified cellulose membrane with good dispersion of vanadium oxide;

[0065] (4) 1 g PMMA and 0.6 g lithium salt (LiDFOB) were mixed evenly, 20 mL N,N-dimethylamide was added, and mechanical stirring was carried out at 60 ° C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0066] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper and dried at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0067] Example 6

[0068] The liquid metal halide used in this embodiment is titanium tetrachloride solution (TiCl4, 0.2mL); the polymer substrate is polyacrylonitrile (PAN), and the lithium salt is lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4). The mass ratio of LiPF6 and LiBF4 is 1:1, and the mass of the lithium salt is 50% of the mass of PAN; the thickness of the polymer solid electrolyte membrane and the thickness of the modified diaphragm are 8:1; the coating density of the polymer solid electrolyte membrane is 60%.

[0069] The specific steps are as follows:

[0070] (1) Dry the hydroxyl-modified polypropylene membrane in a vacuum oven at 80° C. for 24 h, and then completely immerse the membrane in 20 mL of carbon dichloride solvent;

[0071] (2) Add 0.2 mL of titanium tetrachloride solution to the above carbon dichloride solvent and react at 25° C. for 20 h;

[0072] (3) taking out the hydroxyl-modified polypropylene diaphragm and drying it in a vacuum oven at 80° C. for 24 h to obtain a hydroxyl-modified polypropylene diaphragm with good TiO2 dispersion;

[0073] (4) 1 g PAN and 0.5 g lithium salt (LiPF6, LiBF4) were mixed evenly, 20 mL N-methylpyrrolidone was added, and mechanical stirring was carried out at 60 ° C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0074] The polymer electrolyte precursor is uniformly coated on the modified diaphragm with a scraper and dried at 80° C. After drying, a diaphragm-modified solid electrolyte membrane is obtained.

[0075] Example 7

[0076] The liquid metal halide used in this embodiment is titanium tetrachloride solution (TiCl4, 2mL); the polymer substrate is polyvinyl chloride (PVC), and the lithium salt is lithium bis(trifluoromethylsulfonyl)amide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI). The mass ratio of LiTFSI to LiFSI is 1:1, and the mass of the lithium salt is 40% of the mass of PEO; the thickness ratio of the polymer solid electrolyte membrane to the modified diaphragm is 5:1; the coating density of the polymer solid electrolyte membrane is 75%. The thickness of the cellulose porous diaphragm used in this embodiment is 45μm, and the porosity is 38%.

[0077] The specific steps are as follows:

[0078] (1) Dry the cellulose porous membrane in a vacuum oven at 80° C. for 24 h, and then completely immerse the membrane in 20 mL of n-hexane solvent;

[0079] (2) Add 2 mL of titanium tetrachloride solution to the above n-hexane solvent and react at 25° C. for 4 h;

[0080] (3) taking out the cellulose membrane and drying it in a vacuum oven at 80° C. for 24 h to obtain a modified cellulose membrane with good TiO2 dispersion;

[0081] (4) 1 g of PVC and 0.4 g of lithium salt (LiTFSI, LiFSI) were mixed evenly, 20 mL of tetrahydrofuran was added, and mechanical stirring was carried out at 60 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0082] The polymer electrolyte precursor is uniformly coated on the modified cellulose separator with a scraper and dried at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0083] Example 8

[0084] The liquid metal halide used in this embodiment is titanium tetrachloride solution (TiCl4, 2mL); the polymer substrate is polyvinyl chloride (PVC), and the lithium salt is lithium bis(trifluoromethylsulfonyl)amide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI). The mass ratio of LiTFSI to LiFSI is 1:1, and the mass of the lithium salt is 30% of the mass of PEO; the thickness ratio of the polymer solid electrolyte membrane to the modified diaphragm is 5:1; the coating density of the polymer solid electrolyte membrane is 70%.

[0085] The specific steps are as follows:

[0086] (1) Dry the hydroxyl-modified polyethylene membrane in a vacuum oven at 80° C. for 24 h, and then completely immerse the membrane in 20 mL of p-xylene solvent;

[0087] (2) Add 2 mL of titanium tetrachloride solution to the above-mentioned p-xylene solvent and react at 25° C. for 4 h;

[0088] (3) taking out the hydroxyl-modified polyethylene membrane and drying it in a vacuum oven at 80° C. for 24 h to obtain a hydroxyl-modified polyethylene membrane with good TiO2 dispersion;

[0089] (4) 1 g of PVC and 0.3 g of lithium salt (LiTFSI, LiFSI) were mixed evenly, 20 mL of tetrahydrofuran was added, and mechanical stirring was carried out at 60 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0090] The polymer electrolyte precursor is uniformly coated on the modified diaphragm with a scraper and dried at 80° C. After drying, a diaphragm-modified solid electrolyte membrane is obtained.

[0091] Comparative Example 1

[0092] In this comparative example, the polymer substrate is polyvinylidene fluoride (PVDF), and the lithium salt is lithium bis(oxalatoborate) (LiBOB), the mass of the lithium salt is 50% of the mass of PVDF; the polymer solid electrolyte membrane is 1 / 2 of the thickness of the diaphragm; the coating density of the polymer solid electrolyte membrane is 75%. The thickness of the cellulose porous diaphragm used in this embodiment is 45 μm, and the porosity is 38%. The scanning image of the unmodified cellulose diaphragm is shown in Figure 3 .

[0093] The specific steps are as follows:

[0094] 1 g PVDF and 0.5 g lithium salt (LiBOB) were mixed evenly, 20 mL tetrahydrofuran was added, and mechanical stirring was performed at 25 °C for 24 h to obtain a polymer electrolyte precursor with good fluidity;

[0095] The polymer electrolyte precursor is uniformly coated on the cellulose separator with a scraper and dried at 80° C. After drying, a separator-modified solid electrolyte membrane is obtained.

[0096] Figure 1 is a scan of the modified cellulose membrane prepared in Example 2; Figure 1 It can be seen that the hydroxyl groups on the cellulose surface react with boron chloride, and the generated nano-boron oxide particles cover the cellulose surface;

[0097] Figure 2 IT curve of the solid electrolyte membrane composed of the PVDF polymer and the cellulose membrane modified by nano boron oxide particles prepared in Example 2. The lithium ion transference number is 0.58.

[0098] Figure 4This is the IT curve of the solid electrolyte membrane composed of PVDF polymer and unmodified cellulose membrane prepared in Comparative Example 1, and the lithium ion migration number is only 0.20.

[0099] The elastic modulus of the solid electrolyte membrane composed of PVDF polymer and unmodified cellulose membrane prepared in Comparative Example 1 is 12.4 MPa, and the elastic modulus of the solid electrolyte membrane composed of PVDF polymer and cellulose membrane modified by nano boron oxide particles prepared in Example 2 is 26.8 MPa, which effectively improves the high migration number and good mechanical properties of the solid electrolyte membrane.

[0100] The hydroxyl-modified polyethylene diaphragm or the hydroxyl-modified polypropylene diaphragm can be prepared by the method of the prior art, for example, by the method of Chinese patent CN102888016B.

[0101] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0102] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a modified diaphragm, characterized in that: Prepared according to the following steps: The hydroxyl-rich membrane is immersed in an organic solvent A, and a liquid metal halide is added. At room temperature, the hydroxyl group and the halogen element react to form a metal oxide to obtain a modified membrane; the volume ratio of the organic solvent A to the liquid metal halide is 5-200:1, and the reaction time is 4-24h; The hydroxyl-rich membrane is a cellulose porous membrane, a hydroxyl-modified polyethylene membrane or a hydroxyl-modified polypropylene membrane.

2. The method for preparing a modified diaphragm according to claim 1, characterized in that: The organic solvent A is one of n-hexane, toluene, carbon dichloride and p-xylene.

3. The method for preparing a modified diaphragm according to claim 1, characterized in that: Liquid metal halides include, but are not limited to, titanium tetrachloride, boron trichloride, vanadium tetrachloride, and tin tetrachloride.

4. A modified diaphragm prepared by the preparation method according to any one of claims 1 to 3.

5. A solid electrolyte based on the modified diaphragm according to claim 4, characterized in that: The invention comprises a modified diaphragm and a polymer solid electrolyte membrane, wherein the thickness ratio of the polymer solid electrolyte membrane to the modified diaphragm is (1:10) to (10:1); the coating density of the polymer solid electrolyte membrane is 50-99%; The polymer solid electrolyte membrane is composed of a polymer substrate and a lithium salt, wherein the lithium salt accounts for 20% to 80% of the mass of the polymer substrate; The solid electrolyte based on the modified separator was prepared according to the following steps: The polymer substrate and lithium salt are dissolved in an organic solvent B, stirred evenly and then coated on the modified diaphragm, and vacuum dried to obtain a solid electrolyte based on the modified diaphragm.

6. The solid electrolyte based on the modified diaphragm according to claim 5, characterized in that: The polymer substrate is selected from one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene oxide-polypropylene oxide-polyethylene oxide, polymethyl methacrylate, polyacrylonitrile, and polyvinyl chloride.

7. The solid electrolyte based on the modified diaphragm according to claim 5, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)amide, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate and lithium dioxalatoborate.

8. The solid electrolyte based on the modified diaphragm according to claim 5, characterized in that: The organic solvent B is one of tetrahydrofuran, acetonitrile, N,N-dimethylformamide, N-methylpyrrolidone and acetone.