Flame retardant polypropylene composite film and preparation method and application thereof

The flame-retardant polypropylene composite film prepared by multi-layer co-extrusion method combines homopolymer polypropylene, impact copolymer, polyolefin elastomer and flame retardant to solve the problem of insufficient impact and flame retardant properties of polypropylene film. A high-performance polypropylene composite film was realized.

CN115991023BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111221972.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-10-15
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

It is difficult for existing polypropylene films to have good impact resistance and flame retardant properties at the same time, and its flame resistance is poor, which limits its use in industries such as electrical appliances, chemicals, machinery, and military products.

Method used

A multi-layer co-extrusion method is used to prepare a flame-retardant polypropylene composite film, which includes a multi-layer structure film composed of homopolymer polypropylene, propylene impact copolymer, polyolefin elastomer, random polypropylene and flame retardant. Proportional and hierarchical structure to improve the impact resistance, tensile and flame retardant properties of the film.

Benefits of technology

The polypropylene composite film has good heat sealing strength, impact resistance and flame retardant properties at a lower heat sealing temperature. The longitudinal tensile strength is ≥38MPa, the oxygen index is ≥22%, and the pendulum impact strength is ≥0.4J, 150 Heat sealing strength at ℃ ≥15N/15mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003312941210000211
    Figure BDA0003312941210000211
  • Figure BDA0003312941210000221
    Figure BDA0003312941210000221
Patent Text Reader

Abstract

The present invention belongs to the field of films, and relates to a flame-retardant polypropylene composite film, a preparation method thereof, and an application thereof. The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A, at least one film layer B formed by a polypropylene composition B, and at least one film layer C formed by a polypropylene composition C; wherein the polypropylene composition A comprises homopolymerized polypropylene a, propylene impact copolymer b, and polyolefin elastomer c, the polypropylene composition B comprises random polypropylene x and an optional polyolefin elastomer y, and the polypropylene composition C comprises polypropylene m and a flame retardant n. The composite film of the present invention has good impact resistance, tensile properties, and flame retardant properties at the same time, and has good heat sealing strength at a relatively low heat sealing temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of films, and in particular relates to a flame-retardant polypropylene composite film and a preparation method and application thereof. Background Art

[0002] Polypropylene film can usually be made by casting and biaxial stretching, but the impact strength of polypropylene film made from homopolymer polypropylene raw materials is usually low. Polypropylene film is often used for packaging purposes, and the film needs to have high impact performance. To improve the impact performance of polypropylene film, block impact polypropylene can be used to prepare the film, or polyolefin elastomer can be added to polypropylene, but the film prepared by the above methods usually has a high haze. It is also possible to add a nucleating agent to the film at the same time to reduce the haze of the film by refining the crystals in the film, but this method will lead to a decrease in impact performance.

[0003] In order to improve the impact resistance and toughness of the film, the film can also be prepared by a multi-layer co-extrusion method. For example, CN101913279A uses a three-layer co-extrusion method to prepare a composite film. The middle layer of the film is an elastomer and PP blended in a ratio of 1:10-1:3. The elastomer provides good impact resistance. However, this method has the problem of difficulty in uniform dispersion when the elastomer content is high, and the amount of elastomer added will be limited, because when the amount added reaches a certain level, phase separation will occur, thereby limiting the further improvement of impact performance. Moreover, when the film is used for packaging purposes, it is usually hoped that it has good heat sealing performance at a lower heat sealing temperature.

[0004] Polypropylene has poor flame retardancy and a low oxygen index of only 17.0-17.5%. It is a flammable material. When burning, it has a high heat release rate and high calorific value, and is very easy to spread flames and cause fires. These have greatly limited the use of polypropylene film products in industries such as electrical appliances, chemicals, machinery, and military products. Therefore, how to improve the flame retardancy of polymers has also attracted widespread attention. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the existing polypropylene film is difficult to have good impact resistance and flame retardant properties at the same time, and to provide a flame retardant polypropylene composite film and a preparation method thereof. The polypropylene film has good impact resistance, tensile properties and flame retardant properties at the same time, and has good heat sealing strength at a lower heat sealing temperature.

[0006] The first aspect of the present invention provides a flame-retardant polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A, at least one film layer B formed by a polypropylene composition B, and at least one film layer C formed by a polypropylene composition C; wherein the polypropylene composition A comprises homopolymerized polypropylene a, a propylene impact copolymer b, and a polyolefin elastomer c, the polypropylene composition B comprises random polypropylene x and an optional polyolefin elastomer y, and the polypropylene composition C comprises polypropylene m and a flame retardant n.

[0007] The second aspect of the present invention provides a method for preparing the flame-retardant polypropylene composite film, comprising: extruding and casting a raw material composition for forming each layer after an optional granulation process to form the composite film.

[0008] The third aspect of the present invention provides application of the flame retardant polypropylene composite film in the field of packaging materials.

[0009] The composite film of the present invention has good impact resistance, tensile properties and flame retardant properties, and has good heat sealing strength at a relatively low heat sealing temperature. The longitudinal (MD) tensile strength of the film is ≥38MPa, preferably ≥45MPa. The pendulum impact strength is ≥0.4J, preferably ≥0.9J. The heat sealing strength at 150°C is ≥15N / 15mm, preferably ≥18N / 15mm. The oxygen index of the film is ≥22%, preferably ≥23%.

[0010] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0011] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0012] The present invention provides a flame-retardant polypropylene composite film, which comprises at least one film layer A formed by a polypropylene composition A, at least one film layer B formed by a polypropylene composition B, and at least one film layer C formed by a polypropylene composition C; wherein the polypropylene composition A comprises homopolypropylene a, propylene impact copolymer b and polyolefin elastomer c, the polypropylene composition B comprises random polypropylene x and optional polyolefin elastomer y, and the polypropylene composition C comprises polypropylene m and a flame retardant n.

[0013] According to some embodiments of the present invention, a rubber phase is present in the composite film, and the average width of the rubber phase is 20-200 nm, and the average aspect ratio is 5-20. The rubber phase can be observed by atomic force microscopy and is in the shape of a strip. The meaning of the aspect ratio is well known to those skilled in the art. For the test of strip-shaped particles, the aspect ratio is the same as the concept of the length-to-width ratio, that is, the ratio of the longest diameter passing through the inside of the particle to the longest diameter perpendicular to it. The former also corresponds to the length of the particle, and the latter corresponds to the width of the particle.

[0014] According to some embodiments of the present invention, the polypropylene composite film has at least one of the following characteristics: longitudinal (MD) tensile strength ≥38MPa, preferably longitudinal (MD) tensile strength ≥45MPa; oxygen index ≥22%, preferably oxygen index ≥23%; pendulum impact strength ≥0.4J, preferably pendulum impact strength ≥0.9J; heat sealing strength at 150°C ≥15N / 15mm; preferably heat sealing strength at 150°C ≥18N / 15mm.

[0015] According to some embodiments of the present invention, the homopolypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of greater than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.0. Homopolypropylene meeting the above characteristics is commercially available. For example, homopolypropylene with a grade of PPH-FA03 of Qingdao Refining and Chemical, homopolypropylene with a grade of PPH-FA03 of Zhongyuan Petrochemical, and homopolypropylene with a grade of FC801 of Shanghai Petrochemical. Alternatively, it can be prepared by conventional methods in the art.

[0016] According to the present invention, the propylene impact copolymer is preferably a propylene impact copolymer containing ethylene units, and the propylene impact copolymer comprises an elastic part, which is a copolymer part containing ethylene units, preferably selected from an ethylene-propylene copolymer part and an ethylene-butene copolymer part.

[0017] Preferably, the propylene impact copolymer comprises a propylene homopolymer part and the copolymer part containing ethylene units. The propylene homopolymer part may comprise an isotactic polymer structure.

[0018] Based on the total weight of the propylene impact copolymer b, the content of the copolymerized part containing ethylene units in the propylene impact copolymer b is preferably 3-15wt%. 13 C NMR determination.

[0019] The ethylene content of the propylene impact copolymer b is preferably 1-12 wt%, based on the total weight of the propylene impact copolymer b.

[0020] The propylene impact copolymer b preferably has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

[0021] The propylene impact copolymer may have a block structure or include a propylene block copolymer.

[0022] Propylene impact copolymers meeting the above characteristics are commercially available, such as propylene impact copolymers with the brand name EP200K from Sinopec, propylene impact copolymers with the brand name M180R from Shanghai Petrochemical, and propylene impact copolymers with the brand name PPB-M02D from Maoming Petrochemical. Alternatively, they can be prepared by conventional methods in the art.

[0023] According to some embodiments of the present invention, the polyolefin elastomer c is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0024] According to some embodiments of the present invention, the polyolefin elastomer y is an elastomeric copolymer of ethylene and an alpha olefin, wherein the alpha olefin is preferably C3-C 12 The alpha olefin is more preferably at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

[0025] The polyolefin elastomers meeting the above characteristics are commercially available, for example, polyolefin elastomers with the trademark of Exxon 6102, polyolefin elastomers with the trademark of Mitsui & Co., Ltd., and polyolefin elastomers with the trademark of Exxon EXACT 3139. Alternatively, they can be prepared by conventional methods in the art.

[0026] According to some embodiments of the present invention, the random polypropylene x is a copolymer of propylene and ethylene and / or butene, that is, at least one of a copolymer of propylene and ethylene, a copolymer of propylene and butene, and a copolymer of propylene and ethylene and butene, preferably selected from at least one of an ethylene-propylene-butene terpolymer, a propylene-ethylene binary random copolymer, and a propylene-butene binary random copolymer.

[0027] The melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is preferably 2-10 g / 10 min.

[0028] Random polypropylenes meeting the above characteristics are commercially available, such as Yanshan Petrochemical's F5006 random polypropylene, Shanghai Petrochemical's F500EPS random polypropylene, and Shanghai Petrochemical's F800EPS random polypropylene. Alternatively, they can be prepared by conventional methods in the art.

[0029] The film layer C of the present invention mainly exists as a flame retardant functional layer. Therefore, the polypropylene m in the polypropylene composition C can be various types of polypropylene. Preferably, its composition is the same as the following components, compositions or mixtures thereof: homopolymer polypropylene a, random polypropylene x, polypropylene composition A, polypropylene composition B, for example, the same as the composition of a mixture of polypropylene composition A and polypropylene composition B.

[0030] The present invention does not particularly limit the type of the flame retardant. Preferably, the flame retardant is selected from at least one of metal or non-metal hydroxides and / or hydrates of oxides, phosphorus flame retardants, boron flame retardants, antimony flame retardants and intumescent flame retardants. The hydrate of the metal or non-metal hydroxide and / or oxide may be at least one of the hydroxides of aluminum, magnesium, boron, zinc and layered double metal hydroxides; the phosphorus flame retardant may be at least one of red phosphorus, phosphate, polyphosphate and phosphate ester; the boron flame retardant may be boric acid and / or borate, and the borate is preferably ammonium borate and / or zinc borate; the antimony flame retardant may be at least one of antimony trioxide, antimony pentoxide and sodium antimonate; the intumescent flame retardant may be sulfuric acid, pentaerythritol or its dimer or trimer, butanethritol, cyclohexane hexol, sorbitol, glucose, maltose, starch, resorcinol, ammonium polyphosphate, dicyandiamide, melamine, urea, melamine, glycine, expandable graphite and carbon nanotubes. According to a specific embodiment of the present invention, the flame retardant is an intumescent flame retardant, preferably ammonium polyphosphate and pentaerythritol, specifically, the weight ratio of ammonium polyphosphate to pentaerythritol is 0.5-5:1. According to another specific embodiment of the present invention, the flame retardant is a mixture of magnesium hydroxide and aluminum hydroxide, specifically, the weight ratio of magnesium hydroxide to aluminum hydroxide is 0.5-2: 1. The flame retardant polypropylene film prepared by adding the flame retardant has the advantages of easy processing and good performance.

[0031] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 40-90 wt% of homopolypropylene a, 5-45 wt% of propylene impact copolymer b and 2-40 wt% of polyolefin elastomer c.

[0032] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 55-75 wt% homopolypropylene a, 10-30 wt% propylene impact copolymer b and 5-20 wt% polyolefin elastomer c.

[0033] Since homopolymerized polypropylene contains relatively large spherulites, and propylene impact copolymer and polyolefin elastomer contain rubber phases of different sizes, each component will have a common influence. According to the research of the inventors, according to the composition provided by the present invention, the size of the rubber phase in the composition can absorb impact energy well, meet the requirements of impact performance, and make the film have good impact performance. At the same time, since the macromolecular chain segments of the homopolymer phase are relatively regular, crystallization occurs during the film preparation process, so the film also has good tensile properties.

[0034] According to some embodiments of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-100 wt % of the random polypropylene x and 0-60 wt % of the polyolefin elastomer y.

[0035] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 75-90 wt% of the random polypropylene x and 10-25 wt% of the polyolefin elastomer y.

[0036] Polyolefin elastomer can improve the impact performance of the film, but when added in large amounts, it will separate from the matrix, resulting in decreased mechanical properties. According to the composition B provided by the present invention, the heat sealing strength of the film can be improved.

[0037] According to some embodiments of the present invention, based on the total weight of the polypropylene composition C, the polypropylene composition C includes 30-80 wt% of the polypropylene m and 20-70 wt% of the flame retardant n.

[0038] According to a preferred embodiment of the present invention, based on the total weight of the polypropylene composition C, the polypropylene composition C comprises 40-70 wt% of polypropylene m and 30-60 wt% of flame retardant n.

[0039] According to some embodiments of the present invention, based on the total weight of the polypropylene composition A as 100 parts by weight, the weight of the polyolefin elastomer c is calculated as Wc, based on the total weight of the polypropylene composition B as 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wc to Wy is 6:1-1:4, for example, it can be 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5 and any value therebetween.

[0040] According to a preferred embodiment of the present invention, the ratio of Wc to Wy is 1:1-1:2.

[0041] According to the research conducted by the present inventors, when a multi-layer film is co-extruded, when the ratio of Wc to Wy is within the range of the present invention, the impact performance of the film can be further improved, and at the same time the extrusion process will be more stable.

[0042] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min, preferably 2-7 g / 10 min.

[0043] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 2-10 g / 10 min, preferably 3-8 g / 10 min.

[0044] According to some embodiments of the present invention, at 230° C. and under a load of 2.16 kg, the melt mass flow rate of the polypropylene composition C is 2-10 g / 10 min, preferably 2-7 g / 10 min.

[0045] When the melt mass flow rates of the polypropylene composition A, the polypropylene composition B and the polypropylene composition C are within the above range, the film preparation process can be made smoother, thereby ensuring that the film has better uniformity and mechanical properties.

[0046] The composite film of the present invention may be a film structure of three or more layers, and the other layers may have the same composition as the film layer A, the film layer B or the film layer C, or may have different compositions from the film layer A, the film layer B or the film layer C, or may be a mixture of a polypropylene composition A, a polypropylene composition B and a polypropylene composition C. The film layer C as a flame retardant functional layer is preferably arranged between the film layer B and the film layer A. When the polypropylene composite film is a three-layer structure, the B layer and the A layer may be located on both sides of the C layer, respectively. When the number of layers of the polypropylene composite film exceeds three, such as five layers, two B layers are used as upper and lower surface layers, two C layers are used as middle layers, and one A layer is used as a core layer.

[0047] According to some embodiments of the present invention, in the polypropylene composite film, the ratio of the sum of the thickness of film layer B, the sum of the thickness of film layer C and the sum of the thickness of film layer A is 0.1-3:0.1-1:1, preferably 0.5-2:0.2-0.6:1. At this ratio, the composite film has good mechanical properties.

[0048] In the present invention, in order to improve the performance of the composite film during processing, the composite film preferably further contains an antioxidant and / or a lubricant, which may be contained in the polypropylene composition A and / or the polypropylene composition B and / or the polypropylene composition C.

[0049] In the present invention, the antioxidant may be any antioxidant commonly used in the art, without particular limitation. For example, it may be antioxidant 1076, antioxidant 1010, antioxidant 168, thioester antioxidants (such as DLTP, DSTP), etc. Based on the total amount of polypropylene composition A, polypropylene composition B or polypropylene composition C as 100 parts by weight, the content of the antioxidant may be 0.1-0.8 parts by weight, preferably 0.2-0.4 parts by weight.

[0050] In the present invention, the lubricant is preferably a PEG lubricant and / or a monoglyceride lubricant. Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the lubricant is 0.01-0.5 parts by weight, preferably 0.05-0.2 parts by weight.

[0051] According to the present invention, in order to improve other properties (such as stability, etc.) of the composite film, the composite film preferably further contains a film-forming aid. The film-forming aid can be selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant, and an anti-adhesive agent (anti-adhesive agent). The specific type of the film-forming aid can be a conventional choice in the art, and will not be repeated here.

[0052] In the present invention, based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the film-forming aid may be 0.01-0.5 parts by weight, preferably 0.05-0.3 parts by weight.

[0053] The present invention also provides a method for preparing the polypropylene composite film, comprising: extruding and casting the raw material composition for forming each layer after an optional granulation process to form the composite film.

[0054] In the preparation method of the present invention, the pelletizing process can generally include: uniformly mixing the components of the polypropylene composition and the optional antioxidant, lubricant and film-forming aid in a high-speed mixer, adding the uniformly mixed materials to a twin-screw extruder for melt mixing and uniform extrusion pelletization, and drying to obtain pellets. The processing temperature of the twin-screw extruder can be controlled to be 170-230°C.

[0055] According to some embodiments of the present invention, the pellets can be processed by extrusion casting. The process of the extrusion casting method may include sending the pellets of different compositions to multiple extruders respectively, and after the pellets are co-extruded and composited through the extruder die, they are sequentially passed through a casting roller, a traction roller, and then trimmed and rolled to obtain the composite film. Among them, the temperature of the extrusion casting can be controlled to 170-230°C, and the temperature of the casting roller can be 10-50°C. The specific process of preparing the film by the extrusion casting method is a commonly used choice in the art and will not be repeated here.

[0056] The obtained composite film can be stretched in a subsequent process, such as biaxial stretching, which can further improve the mechanical properties of the composite film.

[0057] According to one embodiment of the present invention, the polypropylene composition A, the polypropylene composition B and the polypropylene composition C are pelletized, extruded and cast, and optionally stretched to obtain the polypropylene composite film.

[0058] The polypropylene composite film of the present invention can be used in the field of packaging materials, such as high-end packaging fields that require high impact resistance of the film, including but not limited to battery packaging and electronic product packaging.

[0059] The specific embodiments of the present invention are described in detail below by way of examples. It should be understood that the examples described below are only used to illustrate and explain the present invention and are not used to limit the present invention.

[0060] In the following examples and comparative examples:

[0061] The film casting equipment was purchased from Swedish Labtech Company, model LCR400.

[0062] The polypropylene composition and film properties were tested according to the following method, and the film test results are shown in Table 1:

[0063] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, wherein the test temperature is 230°C and the load is 2.16 kg.

[0064] (2) Film tensile strength: measured according to the method specified in GB / T 1040.3-2006.

[0065] (3) Film pendulum impact strength: measured according to the method specified in GB / T 8809-2015.

[0066] (4) Oxygen index: measured in accordance with the method specified in GB / T 2406-2008.

[0067] (5) Film heat seal strength: Measured according to the method specified in QB / T 2358. When preparing the sample, the heat seal temperature is 150°C, the heat seal pressure is 0.2 MPa, and the heat seal time is 3 s.

[0068] (6) Determination method of average width and average aspect ratio of the rubber phase of the film: Using the Dimension FastScan Icon atomic force microscope of Bruker Company of the United States, using the quantitative nanomechanical scanning mode, the cross section of the film sample was scanned and observed, and the width of the rubber phase was measured and counted to obtain the average width (based on 200 sample points). The aspect ratio of the rubber phase is the ratio of its length direction to its width direction. After measurement, calculation and statistics, the average aspect ratio (based on 200 sample points) was obtained.

[0069] (7) Isoregularity: Pass 13 C NMR measurement: The nuclear magnetic resonance spectrometer (NMR) of 400 MHz propylene polymer was measured using the AVANCE III nuclear magnetic resonance spectrometer (NMR) of Bruker Company, Switzerland. 13 C-NMR), where the solvent is deuterated o-dichlorobenzene and the sample concentration is 250 mg sample / 2.5 mL solvent. To prevent oxidative degradation of the sample during dissolution and data collection, 2 mg of 2,6-di-tert-butyl-4-methylphenol antioxidant (BHT) was added to the sample. The sample was dissolved at 140°C and collected. 13 C-NMR, test temperature 125°C, probe size 10 mm, 90° pulse, sampling time AQ 5 s, delay time D1 1 s, scan number 6000 times. The content of diad isotacticity [mm] is taken as the isotacticity.

[0070] (8) Molecular weight distribution (Mw / Mn): Determined by gel permeation chromatography (GPC), using a PL-GPC 220 gel permeation chromatograph produced by Polymer Laboratories, UK, in combination with an IR5 infrared detector. The chromatographic column in the gel permeation chromatograph consisted of three Plgel 10 μm MIXED-B columns connected in series. The solvent and mobile phase were both 1,2,4-trichlorobenzene (containing 0.3 g / 1000 mL of the antioxidant 2,6-di-tert-butyl-p-cresol). The column temperature was 150 °C, and the flow rate was 1.0 mL / min. EasiCal PS-1 narrow distribution polystyrene standard produced by PL was used for universal calibration.

[0071] Example 1

[0072] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0073] (1) Preparation of polypropylene composition A:

[0074] Component a is homopolypropylene with the brand name of PPH-FA03, purchased from Qingdao Refining and Chemical, with a melt mass flow rate of 3.1g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.7; component b is a propylene impact copolymer with the brand name of EP200K, purchased from Zhongsha Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 13wt%, and a melt mass flow rate of 3.2g / 10min; component c is a polyolefin elastomer with the brand name of 6102, purchased from Exxon, and is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 75 parts by weight, the mass fraction Wb of component b is 10 parts by weight, and the mass fraction Wc of component c is 15 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight, based on the sum of the masses of the above-mentioned components a, b and c being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain polypropylene composite pellets, and its melt mass flow rate MFR is tested. A =3.6g / 10min.

[0075] (2) Preparation of polypropylene composition B:

[0076] Component x is a random polypropylene with a grade of F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2g / 10min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene structural unit content of 16wt%. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 75 parts by weight, and the mass fraction Wy of component y is 25 parts by weight. Wc:Wy is 3:5. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =3.2g / 10min.

[0077] (3) Preparation of polypropylene composition C:

[0078] The polypropylene component m is a random polypropylene of grade F5006, purchased from Yanshan Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.2 g / 10 min; the flame retardant n is a composition of ammonium polyphosphate and pentaerythritol, purchased from Jinan Taixing Fine Chemical Co., Ltd. The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wm of component m is 50 parts by weight, the mass fraction Wn of component n is 50 parts by weight, and the weight ratio of ammonium polyphosphate to pentaerythritol in component n is 2:1. The other steps are the same as step (1), and finally a polypropylene composition C pellet is obtained.

[0079] (4) Preparation of composite film:

[0080] The pellets of polypropylene composition A, polypropylene composition B and polypropylene composition C obtained in the above steps (1), (2) and (3) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition C is added to the middle layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the temperature of the casting chill roll is set to 30°C, and the film is rolled up to form a composite film, which is three-layer, and is composed of an upper surface layer (film layer B), an intermediate layer (film layer C) and a core layer (film layer A) in sequence. The film thickness is 60μm, wherein the thickness ratio of the film layer B, the film layer C and the film layer A is 1:1:2.

[0081] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 81 nm, and the average aspect ratio was 10.3.

[0082] Example 2

[0083] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0084] (1) Preparation of polypropylene composition A:

[0085] Component a is homopolypropylene with the brand name PPH-FA03, purchased from Zhongyuan Petrochemical, with a melt mass flow rate of 3.0g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.6; component b is a propylene impact copolymer with the brand name M180R, purchased from Shanghai Petrochemical, with an ethylene content of 11wt%, an ethylene-propylene copolymer content of 15wt%, and a melt mass flow rate of 2.0g / 10min; component c is a polyolefin elastomer with the brand name DF640, purchased from Mitsui Co., Ltd., and is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wa of component a is 65 parts by weight, the mass fraction Wb of component b is 30 parts by weight, and the mass fraction Wc of component c is 5 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned components a, b and c being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =3.2g / 10min.

[0086] (2) Preparation of polypropylene composition B:

[0087] Component x is a random polypropylene with the brand name F500EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 5.3g / 10min; component y is a polyolefin elastomer with the brand name DF640, purchased from Mitsui & Co., Ltd., which is an ethylene-1-butene copolymer with a butene structural unit content of 32wt%. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 90 parts by weight, and the mass fraction Wy of component y is 10 parts by weight. Wc:Wy is 1:2. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =5.2g / 10min.

[0088] (3) Preparation of polypropylene composition C:

[0089] The polypropylene component m is the polypropylene composition B obtained in the above step (2); the flame retardant n is a composition of ammonium polyphosphate and pentaerythritol purchased from Jinan Taixing Fine Chemical Co., Ltd. The above components are weighed and mixed according to the proportion, wherein the mass fraction Wm of component m is 50 parts by weight, the mass fraction Wn of component n is 50 parts by weight, and the weight ratio of ammonium polyphosphate to pentaerythritol in component n is 2:1. The other steps are the same as step (1), and finally a polypropylene composition C pellet is obtained.

[0090] (4) Preparation of composite film:

[0091] The pellets of polypropylene composition A, polypropylene composition B and polypropylene composition C prepared in the above steps (1), (2) and (3) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion casting machine, the polypropylene composition B is added to the upper surface layer extruder of the multi-layer extrusion casting machine, and the polypropylene composition C is added to the middle layer extruder of the multi-layer extrusion casting machine, wherein an inorganic anti-sticking agent (silicon dioxide, the same below) is added to the upper surface layer extruder, and the weight ratio of the anti-sticking agent to the polypropylene composition pellets is 0.2:100. During the casting process, the casting chill roll temperature is set to 30°C, and the film is rolled up to form a composite film, which is composed of upper and lower surface layers (film layer B), two middle layers (film layer C) located on both sides of the core layer, and a core layer (film layer A). The film thickness is 50μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers, the sum of the thickness of the middle layers on both sides of the core layer to the thickness of the core layer is 2:1:2.

[0092] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 69 nm, and the average aspect ratio was 13.2.

[0093] Example 3

[0094] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0095] (1) Preparation of polypropylene composition A:

[0096] Component a is a homopolymer polypropylene with a brand name of FC801, purchased from Shanghai Petrochemical, with a melt mass flow rate of 7.8g / 10min, an isotacticity of 98%, and a molecular weight distribution Mw / Mn of 4.8; component b is a propylene impact copolymer with a brand name of PPB-M02D, purchased from Maoming Petrochemical, with an ethylene content of 8wt%, an ethylene-propylene copolymer content of 10wt%, and a melt mass flow rate of 1.5g / 10min; component c is a polyolefin elastomer with a brand name of EXACT3139, purchased from Exxon, and is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%. The above-prepared components are weighed and mixed according to a ratio, wherein the mass fraction Wa of component a is 55 parts by weight, the mass fraction Wb of component b is 25 parts by weight, and the mass fraction Wc of component c is 20 parts by weight. Then, a lubricant is added (the lubricant is a PEG lubricant produced by Clariant of Switzerland, with a molecular weight of 10,000, and the amount of the lubricant added is 0.1 parts by weight based on the sum of the masses of the above-mentioned components a, b and c being 100 parts by weight), and then the mixture is added to a high-speed stirrer for uniform mixing, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 160-230° C. The screw is melt-mixed uniformly, extruded, granulated and dried to obtain pellets of a polypropylene composition A. The melt mass flow rate MFR thereof is tested. A =6.6g / 10min.

[0097] (2) Preparation of polypropylene composition B:

[0098] Component x is a random polypropylene with the brand name F800EPS, purchased from Shanghai Petrochemical, which is an ethylene-propylene-butene terpolymer with a melt mass flow rate of 8.2g / 10min; component y is a polyolefin elastomer with the brand name EXACT3139, purchased from Exxon, which is an ethylene-1-octene copolymer with an octene structural unit content of 14wt%. The above-prepared components are weighed and mixed according to the ratio, wherein the mass fraction Wx of component x is 80 parts by weight, and the mass fraction Wy of component y is 20 parts by weight. Wc:Wy is 1:1. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained. The melt mass flow rate MFR B =7.9g / 10min.

[0099] (3) Preparation of polypropylene composition C:

[0100] The same as Example 2, except that the polypropylene component m is the polypropylene composition B obtained in the above step (2), and finally the polypropylene composition C pellets are obtained.

[0101] (4) Preparation of composite film:

[0102] The preparation process is the same as step (4) of Example 1.

[0103] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 95 nm, and the average aspect ratio was 9.6.

[0104] Example 4

[0105] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0106] (1) Preparation of polypropylene composition A:

[0107] The steps are the same as those in Example 1. The difference is that the mass fraction Wa of component a is 80 parts by weight, the mass fraction Wb of component b is 18 parts by weight, and the mass fraction Wc of component c is 2 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR is tested. A =2.8g / 10min.

[0108] (2) Preparation of polypropylene composition B:

[0109] The steps are the same as those in Example 1. The difference is that the mass fraction Wx of component x is 92 parts by weight, and the mass fraction Wy of component y is 8 parts by weight. Wc:Wy is 1:4. The other steps are the same as those in step (1), and finally a pellet of polypropylene composition B is obtained. The melt mass flow rate MFR thereof is tested. B =7.7g / 10min.

[0110] (3) Preparation of polypropylene composition C:

[0111] The steps are the same as those of Example 2, except that the polypropylene component m is the polypropylene composition B obtained in the above step (2), and finally the polypropylene composition C pellets are obtained.

[0112] (4) Preparation of composite film:

[0113] The steps are the same as those in Example 1. The film thickness is 60 μm, wherein the thickness ratio of the film layer B, the film layer C and the film layer A is 1:1:3.

[0114] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 105 nm, and the average aspect ratio was 8.7.

[0115] Example 5

[0116] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0117] (1) Preparation of polypropylene composition A:

[0118] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 90 parts by weight, the mass fraction Wb of component b is 5 parts by weight, and the mass fraction Wc of component c is 5 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR A =9.6g / 10min.

[0119] (2) Preparation of polypropylene composition B:

[0120] The steps are the same as in Example 3.

[0121] (3) Preparation of polypropylene composition C:

[0122] The steps are the same as those in Example 2, the polypropylene component m is the polypropylene composition B obtained in the above step (1), the mass fraction Wm of component m is 65 parts by weight, and the mass fraction Wn of component n is 35 parts by weight, and finally polypropylene composition C pellets are obtained.

[0123] (4) Preparation of composite film:

[0124] The steps are the same as those in Example 2. The film thickness is 60 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers, the sum of the thickness of the intermediate layers on both sides of the core layer, and the thickness of the core layer is 2:1:1.

[0125] Example 6

[0126] This example is used to illustrate the preparation of the polypropylene composite film provided by the present invention.

[0127] (1) Preparation of polypropylene composition A:

[0128] The steps are the same as those in Example 3, except that the mass fraction Wa of component a is 50 parts by weight, the mass fraction Wb of component b is 40 parts by weight, and the mass fraction Wc of component c is 10 parts by weight. The polypropylene composition A pellets are obtained, and the melt mass flow rate MFR A =4.6g / 10min.

[0129] (2) Preparation of polypropylene composition B:

[0130] The steps are the same as those in Example 3, except that the mass fraction Wx of component x is 60 parts by weight, and the mass fraction Wy of component y is 40 parts by weight. Wc:Wy is 1:4. Finally, the polypropylene composition B pellets are obtained, and the melt mass flow rate MFR is tested. B =9.8g / 10min.

[0131] (3) Preparation of polypropylene composition C:

[0132] The steps are the same as those of Example 3, except that the polypropylene component m is the polypropylene composition B obtained in the above step (2), and finally the polypropylene composition C pellets are obtained.

[0133] (4) Preparation of composite film:

[0134] The steps are the same as those in Example 3. The film thickness is 60 μm, wherein the ratio of the sum of the thickness of the upper and lower surface layers, the sum of the thickness of the intermediate layers on both sides of the core layer, and the thickness of the core layer is 1:1:4.

[0135] Example 7

[0136] A polypropylene composite film was prepared according to the method of Example 1. The difference was that in the preparation of the polypropylene composition C, the flame retardants ammonium polyphosphate and pentaerythritol were replaced by magnesium hydroxide and aluminum hydroxide. The mass fraction Wm of component m was 50 parts by weight, the mass fraction Wn of component n was 50 parts by weight, and the weight ratio of magnesium hydroxide to aluminum hydroxide in component n was 1:1.

[0137] Example 8

[0138] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 40 parts by weight, the mass fraction Wb of component b is 40 parts by weight, and the mass fraction Wc of component c is 20 parts by weight. Wc:Wy is 4:5. The pellets of the polypropylene composition A were obtained, and the melt mass flow rate MFR A =2.8g / 10min.

[0139] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 140 nm, and the average aspect ratio was 7.1.

[0140] Example 9

[0141] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 50 parts by weight, the mass fraction Wb of component b is 45 parts by weight, and the mass fraction Wc of component c is 5 parts by weight. Wc:Wy is 1:5. The pellets of the polypropylene composition A were obtained, and the melt mass flow rate MFR A =3.1g / 10min.

[0142] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 176 nm, and the average aspect ratio was 6.4.

[0143] Example 10

[0144] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of the polypropylene composition A, the mass fraction Wa of component a is 50 parts by weight, the mass fraction Wb of component b is 10 parts by weight, and the mass fraction Wc of component c is 40 parts by weight. Wc:Wy is 8:5. The pellets of the polypropylene composition A were obtained, and the melt mass flow rate MFR A =2.7g / 10min.

[0145] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 150 nm, and the average aspect ratio was 6.8.

[0146] Embodiment 11

[0147] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 50 parts by weight, and the mass fraction Wy of component y is 50 parts by weight. Wc:Wy is 3:10. The pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR was tested. B =4.7g / 10min.

[0148] The composite film was observed under an atomic force microscope, and a rubber phase was visible. The average width of the rubber phase was 98 nm, and the average aspect ratio was 15.1.

[0149] Example 12

[0150] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition B contained only component x.

[0151] Example 13

[0152] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 92.5 parts by weight, and the mass fraction Wy of component y is 7.5 parts by weight. Wc:Wy is 2:1. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR was tested. B =5.5g / 10min.

[0153] Embodiment 14

[0154] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 85 parts by weight, and the mass fraction Wy of component y is 15 parts by weight. Wc:Wy is 1:1. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR B =5.1g / 10min.

[0155] Embodiment 15

[0156] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 70 parts by weight, and the mass fraction Wy of component y is 30 parts by weight. Wc:Wy is 1:2. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR was tested. B =4.4g / 10min.

[0157] Example 16

[0158] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 40 parts by weight, and the mass fraction Wy of component y is 60 parts by weight. Wc:Wy is 1:4. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR was tested. B =2.9g / 10min.

[0159] Embodiment 17

[0160] A polypropylene composite film was prepared according to the method of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 97 parts by weight, and the mass fraction Wy of component y is 3 parts by weight. Wc:Wy is 5:1. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate MFR was tested. B =6.0g / 10min.

[0161] Comparative Example 1

[0162] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the composite film was made of polypropylene composition A and polypropylene composition C, and the composite film consisted of an upper surface layer (film layer C) and a core layer (film layer A). The film thickness was 60 μm, wherein the thickness ratio of film layer C to film layer A was 1:2.

[0163] Comparative Example 2

[0164] A polypropylene composite film was prepared according to the method of Example 2. The difference was that the composite film was made of polypropylene composition B and polypropylene composition C, and the composite film consisted of an upper surface layer (film layer B) and a core layer (film layer C). The film thickness was 60 μm, wherein the thickness ratio of film layer B to film layer C was 2:1.

[0165] Comparative Example 3

[0166] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the composite film was made of polypropylene composition A and polypropylene composition B, and the composite film consisted of an upper surface layer (film layer B) and a core layer (film layer A). The film thickness was 60 μm, wherein the thickness ratio of film layer B to film layer A was 1:2.

[0167] Comparative Example 4

[0168] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition A contained only component b.

[0169] Comparative Example 5

[0170] A polypropylene composite film was prepared according to the method of Example 1. The difference was that the polypropylene composition A contained only component a and component b, wherein the mass fraction Wa of component a was 75 parts by weight, and the mass fraction Wb of component b was 25 parts by weight.

[0171] Table 1

[0172]

[0173]

[0174] It can be concluded from the results of the embodiments in Table 1 that the polypropylene composite film provided by the present invention has good impact resistance and tensile properties at the same time, and has good heat sealing strength and flame retardant properties. The longitudinal (MD) tensile strength of the film of the present invention is ≥38MPa, the oxygen index is ≥22%, the pendulum impact strength is ≥0.4J, and the heat sealing strength at 150°C is ≥15N / 15mm. It can be seen from the preferred embodiments that the longitudinal (MD) tensile strength of the film of the present invention is ≥45MPa, the oxygen index is ≥23%, the pendulum impact strength is ≥0.9J, and the heat sealing strength at 150°C is ≥18N / 15mm. It can be seen from the comparative examples that it is difficult to achieve a balance of various properties by changing the composition ratio of the film layer, and during extrusion casting, the film surface is unstable, and it is difficult to obtain a film with uniform thickness.

[0175] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0176] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A flame retardant polypropylene composite film, characterized in that: The polypropylene composite film comprises at least one film layer A formed by a polypropylene composition A, at least one film layer B formed by a polypropylene composition B, and at least one film layer C formed by a polypropylene composition C; wherein the polypropylene composition A comprises homopolypropylene a, propylene impact copolymer b and polyolefin elastomer c, the polypropylene composition B comprises random polypropylene x and optionally polyolefin elastomer y, and the polypropylene composition C comprises polypropylene m and a flame retardant n; A rubber phase exists in the polypropylene composite film, wherein the average width of the rubber phase is 20-200 nm and the average aspect ratio is 5-20; Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 40-90 wt% of homopolypropylene a, 5-45 wt% of propylene impact copolymer b and 2-40 wt% of polyolefin elastomer c; based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 40-100 wt% of random polypropylene x and 0-60 wt% of polyolefin elastomer y; based on the total weight of the polypropylene composition C, the polypropylene composition C comprises 30-80 wt% of polypropylene m and 20-70 wt% of flame retardant n; When the polypropylene composition B includes the polyolefin elastomer y, based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer c is calculated as Wc, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is calculated as Wy, and the ratio of Wc to Wy is 6:1-1:4; The propylene impact copolymer b is a propylene impact copolymer containing ethylene units; based on the total weight of the propylene impact copolymer b, the ethylene content of the propylene impact copolymer b is 1-12wt%; the polyolefin elastomer c and the polyolefin elastomer y are each independently an elastomeric copolymer of ethylene and alpha olefin.

2. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The polypropylene composite film has at least one of the following characteristics: longitudinal tensile strength ≥38 MPa; oxygen index ≥22%; pendulum impact strength ≥0.4 J; heat sealing strength at 150° C. ≥15 N / 15 mm.

3. The flame-retardant polypropylene composite film according to claim 2, characterized in that: Longitudinal tensile strength ≥45MPa.

4. The flame-retardant polypropylene composite film according to claim 2, characterized in that: Oxygen index ≥23%.

5. The flame-retardant polypropylene composite film according to claim 2, characterized in that: Pendulum impact strength ≥0.9J.

6. The flame-retardant polypropylene composite film according to claim 2, characterized in that: Heat sealing strength at 150°C ≥18N / 15mm.

7. The flame-retardant polypropylene composite film according to claim 1, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 2-10 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition C is 2-10 g / 10 min.

8. The flame-retardant polypropylene composite film according to claim 7, characterized in that: At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition A is 2-7 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition B is 3-8 g / 10 min; At 230° C. and a load of 2.16 kg, the melt mass flow rate of the polypropylene composition C is 2-7 g / 10 min.

9. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The homopolymer polypropylene a has a melt mass flow rate of 2-15 g / 10 min at 230° C. and a load of 2.16 kg, an isotacticity of more than 97%, and a molecular weight distribution Mw / Mn of 4.5-7.

0.

10. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The copolymerization part containing ethylene units in the propylene impact copolymer b has a content of 3-15wt%; The propylene impact copolymer b has a melt mass flow rate of 1-10 g / 10 min at 230° C. and a load of 2.16 kg.

11. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The alpha olefin is C3-C 12 of alpha olefins.

12. The flame-retardant polypropylene composite film according to claim 11, characterized in that: The alpha olefin is at least one selected from propylene, 1-butene, 1-hexene and 1-octene.

13. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The random polypropylene x is a copolymer of propylene and ethylene and / or butene; the melt mass flow rate of the random polypropylene x at 230° C. and a load of 2.16 kg is 2-10 g / 10 min.

14. The flame-retardant polypropylene composite film according to claim 13, characterized in that: The random polypropylene x is at least one selected from ethylene-propylene-butene terpolymer, propylene-ethylene binary random copolymer, and propylene-butene binary random copolymer.

15. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The composition of the polypropylene m is the same as the composition of the following components, compositions or mixtures thereof: homopolypropylene a, random polypropylene x, polypropylene composition A, polypropylene composition B.

16. The flame-retardant polypropylene composite film according to claim 1, characterized in that: The flame retardant is selected from at least one of a hydrate of a metal or non-metal hydroxide and / or oxide, a phosphorus flame retardant, a boron flame retardant, an antimony flame retardant and an intumescent flame retardant.

17. The flame-retardant polypropylene composite film according to claim 16, characterized in that: The hydrate of the metal or non-metal hydroxide and / or oxide is at least one of the hydroxides of aluminum, magnesium, boron, zinc and layered double metal hydroxides; the phosphorus-based flame retardant is at least one of red phosphorus, phosphates, polyphosphates and phosphate esters; the boron-based flame retardant is boric acid and / or borates; the antimony-based flame retardant is at least one of antimony trioxide, antimony pentoxide and sodium antimonate; the intumescent flame retardant is at least two of sulfuric acid, pentaerythritol or its dimer or trimer, butanethritol, cyclohexanehexol, sorbitol, glucose, maltose, starch, resorcinol, ammonium polyphosphate, dicyandiamide, melamine, urea, melamine, glycine, expandable graphite and carbon nanotubes.

18. The flame-retardant polypropylene composite film according to claim 17, characterized in that: The borate is ammonium borate and / or zinc borate.

19. The flame-retardant polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 55-75 wt% of homopolypropylene a, 10-30 wt% of propylene impact copolymer b and 5-20 wt% of polyolefin elastomer c.

20. The flame retardant polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition B, the polypropylene composition B comprises 75-90 wt% of the random polypropylene x and 10-25 wt% of the polyolefin elastomer y.

21. The flame-retardant polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition C, the polypropylene composition C comprises 40-70 wt% of the polypropylene m and 30-60 wt% of the flame retardant n.

22. The flame-retardant polypropylene composite film according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A being 100 parts by weight, the weight of the polyolefin elastomer c is Wc, based on the total weight of the polypropylene composition B being 100 parts by weight, the weight of the polyolefin elastomer y is Wy, and the ratio of Wc to Wy is 1:1-1:

2.

23. The flame retardant polypropylene composite film according to any one of claims 1 to 22, characterized in that: In the polypropylene composite film, the ratio of the sum of the thickness of the film layer B, the sum of the thickness of the film layer C and the sum of the thickness of the film layer A is 0.1-3:0.1-1:

1.

24. The flame-retardant polypropylene composite film according to claim 23, characterized in that: In the polypropylene composite film, the ratio of the sum of the thickness of the film layer B, the sum of the thickness of the film layer C and the sum of the thickness of the film layer A is 0.5-2:0.2-0.6:

1.

25. The flame retardant polypropylene composite film according to any one of claims 1 to 22, characterized in that: The film layer C is disposed between the film layer B and the film layer A.

26. The flame retardant polypropylene composite film according to any one of claims 1 to 22, characterized in that: The polypropylene composition A and / or the polypropylene composition B and / or the polypropylene composition C further comprises an antioxidant and / or a lubricant.

27. The flame retardant polypropylene composite film according to claim 26, characterized in that: The antioxidant is selected from at least one of antioxidant 1076, antioxidant 1010, antioxidant 168 and thioester antioxidants.

28. The flame retardant polypropylene composite film according to claim 26, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the antioxidant is 0.1-0.8 parts by weight.

29. The flame retardant polypropylene composite film according to claim 28, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the antioxidant is 0.2-0.4 parts by weight.

30. The flame retardant polypropylene composite film according to claim 26, characterized in that: The lubricant is a PEG lubricant and / or a monoglyceride lubricant.

31. The flame retardant polypropylene composite film according to claim 26, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the lubricant is 0.01-0.5 parts by weight.

32. The flame retardant polypropylene composite film according to claim 31, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the lubricant is 0.05-0.2 parts by weight.

33. The flame retardant polypropylene composite film according to any one of claims 1 to 22, characterized in that: The polypropylene composition A and / or the polypropylene composition B and / or the polypropylene composition C further comprises a film-forming aid.

34. The flame retardant polypropylene composite film according to claim 33, characterized in that: The film-forming aid is selected from at least one of an anti-halogen agent, a light stabilizer, a heat stabilizer, a colorant, a filler, a lubricant and an anti-sticking agent.

35. The flame retardant polypropylene composite film according to claim 33, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the film-forming aid is 0.01-0.5 parts by weight.

36. The flame retardant polypropylene composite film according to claim 35, characterized in that: Based on 100 parts by weight of the total amount of the polypropylene composition A, the polypropylene composition B or the polypropylene composition C, the content of the film-forming aid is 0.05-0.3 parts by weight.

37. A method for preparing a flame retardant polypropylene composite film according to any one of claims 1 to 36, comprising: The raw material composition for forming each layer is extruded and cast after a granulation process to form the composite film; optionally, the method further comprises stretching the obtained composite film.

38. The preparation method according to claim 37, characterized in that: The stretching is bidirectional stretching.

39. Use of the flame-retardant polypropylene composite film according to any one of claims 1 to 36 in the field of packaging materials.

40. The use according to claim 39, characterized in that The packaging is battery packaging or electronic product packaging.

Citation Information

Patent Citations

  • Toughening type three-layer coextru-laminated film and preparation method thereof

    CN101913279A

  • Polymer membrane and preparation method thereof

    CN105623078A

  • Polyethylene composition and flame retardant film

    CN106554543A

  • Flame-retardant antistatic polypropylene composition, flame-retardant antistatic polypropylene material and preparation method thereof

    CN106995576A

  • Heat sealing layer, CPP film, preparation method thereof and aluminum-plastic film

    CN108943932A