A modified amorphous material and preparation method thereof, negative electrode sheet and sodium ion battery

By coating molecular sieves on amorphous carbon materials to form a core-shell structure, the problem of sodium ion intercalation and side reactions in sodium-ion batteries is solved, achieving efficient battery cycle performance and cost reduction, and is suitable for the application of sodium-ion batteries.

CN115991473BActive Publication Date: 2024-10-01HUNAN LIFANG NEW ENERGY SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211590909.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-01
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries dominate energy storage, leading to increased consumption of lithium resources. Moreover, sodium-ion batteries are incompatible with the graphite layer due to their large sodium ion radius and are difficult to embed, making it difficult to develop non-graphite anodes and amorphous carbon materials. It is difficult to form a stable SEI film on the surface, and there are problems such as easy co-embedding of electrolyte and side reactions, which affects the battery cycle performance.

Method used

Using modified amorphous carbon material, the molecular sieve is crushed and coated on the surface of amorphous carbon to form a core-shell structure. The molecular sieve is used as the outer shell and the amorphous carbon is used as the core. A stable coating is formed through heat treatment to suppress side reactions and improve Battery performance.

Benefits of technology

It achieves high structural stability and cycle stability of the modified amorphous carbon material, improves the first Coulomb efficiency and cycle life, reduces the cost and energy consumption of the battery, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115991473B_ABST
    Figure CN115991473B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of secondary batteries, and in particular, relates to a modified amorphous carbon material, including molecular sieves and amorphous carbon, wherein the modified amorphous carbon material presents a core-shell structure, wherein the outer shell is a molecular sieve and the inner core is amorphous carbon, wherein the amorphous carbon includes soft carbon and hard carbon. The modified amorphous material of the present invention has high structural stability, high capacity and good cycle stability, and can improve the first coulombic efficiency and cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a modified amorphous material and a preparation method thereof, a negative electrode sheet and a sodium ion battery. Background Art

[0002] With the rapid development of automobile electrification, the demand for lithium-ion power batteries is increasing, resulting in increasingly tight supply of lithium resources and high prices. On the other hand, with the rapid advancement of the national "carbon peak, carbon neutrality" strategy, there is an urgent need to develop clean energy based on wind power and photovoltaics. In order to reduce the phenomenon of abandoned light and wind, it is necessary to configure cheap, sustainable and safe energy storage batteries. Since lithium-ion batteries currently dominate energy storage, the rapid development of the energy storage industry has also exacerbated the rapid consumption of lithium resources and the imbalance between supply and demand. Therefore, it is urgent to develop new energy storage batteries based on non-lithium-ion batteries. Sodium-ion batteries have significant advantages such as low cost, abundant resources, good safety and environmental friendliness, and are suitable for large-scale energy storage. However, sodium ions have a large radius and are incompatible with graphite layers, making them difficult to embed in graphite materials. Therefore, it is extremely critical to develop suitable non-graphite negative electrodes.

[0003] Unlike graphite, amorphous carbon materials, including soft carbon and hard carbon, have long-range disorder and short-range ordered structures, large interlayer spacing, and internal pores, which are suitable for the embedding and extraction of sodium ions. However, it is not easy to form a stable SEI film on the surface of amorphous carbon materials, and there are problems such as easy co-embedding of electrolytes and easy reduction and decomposition on the surface, which is not conducive to long-term battery cycles and has a low initial storage efficiency. Therefore, it is necessary to modify the surface to inhibit the occurrence of side reactions and improve the initial storage efficiency and cycle life. Summary of the invention

[0004] One of the purposes of the present invention is to provide a modified amorphous material with high structural stability, high capacity and good cycle stability, and to improve the first coulombic efficiency and cycle life in view of the shortcomings of the prior art.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A modified amorphous carbon material comprises a molecular sieve and amorphous carbon. The modified amorphous carbon material presents a core-shell structure, wherein the outer shell is the molecular sieve and the inner core is the amorphous carbon. The amorphous carbon comprises soft carbon and hard carbon.

[0007] Preferably, the inner core accounts for 90% to 99% of the weight of the modified amorphous carbon material, and the outer shell accounts for 1% to 10% of the weight of the amorphous carbon material.

[0008] The second purpose of the present invention is to provide a method for preparing a modified amorphous material in view of the deficiencies of the prior art, wherein the preparation method is simple and has good controllability.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for preparing a modified amorphous carbon material comprises the following steps:

[0011] Step A1, crushing the molecular sieve;

[0012] Step A2, uniformly mixing the amorphous carbon and the crushed molecular sieve, and coating the molecular sieve on the surface of the amorphous carbon to form a coating layer to obtain composite particles;

[0013] Step A3: heat-treating the composite particles under an inert atmosphere to obtain a modified amorphous carbon material.

[0014] Preferably, the particle size of the molecular sieve after crushing in step A1 is 100 nm to 500 nm.

[0015] Preferably, the thickness of the coating layer in step A2 is 10 nm to 100 nm.

[0016] Preferably, the heat treatment temperature in step A3 is 300-600° C., the heating rate is 1-10° C. / min, and the heat treatment time is 1-5 hours.

[0017] Preferably, the inert atmosphere is one of argon, nitrogen or helium.

[0018] The third object of the present invention is to provide a negative electrode sheet with good electrochemical performance in view of the deficiencies of the prior art.

[0019] In order to achieve the above object, the present invention adopts the following technical solutions:

[0020] A negative electrode sheet comprises the modified amorphous carbon material.

[0021] The fourth object of the present invention is to provide a sodium ion battery with fewer side reactions, high first coulombic efficiency and long cycle life in view of the shortcomings of the prior art.

[0022] In order to achieve the above object, the present invention adopts the following technical solutions:

[0023] A sodium ion battery comprises the above-mentioned negative electrode sheet.

[0024] Compared with the prior art, the beneficial effects of the present invention are: the modified amorphous carbon material of the present invention has a good structure, few side reactions, low energy consumption for preparation, low cost, short cycle, and is conducive to large-scale production. The modified amorphous carbon material of the present invention contains molecular sieves on the surface, which play the role of artificial SEI, can effectively protect the amorphous carbon, and is conducive to achieving a preferred balance among capacity, coulombic efficiency, and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a scanning electron micrograph of the modified hard carbon material prepared in Example 1 of the present invention.

[0026] Figure 2 3 is a charge and discharge curve diagram of the modified hard carbon material prepared in Example 1 of the present invention.

[0027] Figure 3 It is a charge and discharge curve diagram of the original hard carbon material of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be described in further detail below in conjunction with specific implementation modes and the accompanying drawings, but the implementation modes of the present invention are not limited thereto.

[0029] A modified amorphous carbon material comprises a molecular sieve and amorphous carbon. The modified amorphous carbon material presents a core-shell structure, wherein the outer shell is the molecular sieve and the inner core is the amorphous carbon. The amorphous carbon comprises soft carbon and hard carbon.

[0030] Amorphous carbon includes soft carbon and hard carbon, which has long-range disorder and short-range ordered structure, large interlayer spacing, and contains pores, which are suitable for the embedding and extraction of sodium ions. The molecular sieve of the shell can play the role of an artificial SEI membrane, achieve the desolvation effect, prevent the co-embedding of the solvent, and effectively inhibit or reduce the surface side reactions; on the other hand, the molecular sieve can adsorb the moisture and gas generated by the side reactions during the battery cycle, thereby inhibiting the flatulence of the battery, and the inherent voids in the molecular sieve can provide channels for sodium ions, which does not affect the rapid transmission of sodium ions on the surface. Therefore, the modified amorphous carbon material takes into account high capacity, high first coulomb efficiency, and good cycle stability and rate performance. The molecular sieve is a commercial molecular sieve, selected but not limited to at least one of 3A, 4A, 5A, 10Z, 13Z, Y, sodium mordenite, ZSM-5, and TS-1; more preferably, a sodium-containing molecular sieve is selected to provide a pre-sodium effect.

[0031] The amorphous carbon includes commercial soft carbon and hard carbon, selected from but not limited to coal-based soft carbon, asphalt-based soft carbon, biomass-based hard carbon, resin-based hard carbon, and lignin-based hard carbon. The so-called hard carbon refers to carbon that is difficult to graphitize at high temperatures (generally greater than 2000°C), and the so-called soft carbon refers to carbon that can be graphitized at high temperatures. The preparation method of the soft carbon or hard carbon is generally to pyrolyze and carbonize precursors such as coal, asphalt, resin, biomass (such as coconut shell, lignin) at a certain temperature (1000-1500°C) in an inert atmosphere.

[0032] Preferably, the core accounts for 90% to 99% of the weight percentage of the modified amorphous carbon material, and the shell accounts for 1% to 10% of the weight percentage of the amorphous carbon material. Preferably, the core accounts for 90% to 95%, 95% to 98% of the weight percentage of the modified amorphous carbon material, specifically, the core accounts for 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% of the weight percentage of the modified amorphous carbon material. Preferably, the shell accounts for 1% to 4%, 4% to 8%, 8% to 10% of the weight percentage of the amorphous carbon material, specifically, the shell accounts for 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% of the weight percentage of the amorphous carbon material. Existing carbon materials do not have the core-shell structure of the present invention, and the coating layer is easy to fall off during use, resulting in poor performance. The modified amorphous carbon material of the present invention can form a firm and stable coating layer that is not easy to fall off, thereby improving the cycle performance.

[0033] The second purpose of the present invention is to provide a method for preparing a modified amorphous material in view of the deficiencies of the prior art, wherein the preparation method is simple and has good controllability.

[0034] In order to achieve the above object, the present invention adopts the following technical solutions:

[0035] A method for preparing a modified amorphous carbon material comprises the following steps:

[0036] Step A1, crushing the molecular sieve;

[0037] Step A2, uniformly mixing the amorphous carbon and the crushed molecular sieve, and coating the molecular sieve on the surface of the amorphous carbon to form a coating layer to obtain composite particles;

[0038] Step A3: heat-treating the composite particles under an inert atmosphere to obtain a modified amorphous carbon material.

[0039] The preparation method of the modified amorphous carbon material of the present invention is simple, easy to operate, has low energy consumption, and is easy to operate and control. The crushing includes sand milling, ball milling, and air flow crushing. Preferably, the crushing method is sand milling; wherein the surface coating method is selected from atomic layer deposition, sol-gel method, magnetron sputtering method, and mechanical fusion method; more preferably, the surface coating method is selected from mechanical fusion method, which can achieve uniform, complete, and conformal coating, and has a simple process and low cost, and can achieve large-scale production. The so-called conformal coating refers to the coating material and the coated material being highly consistent in morphology and texture. During the mechanical fusion process, the morphology and particle size of the coated material remain unchanged, and the coating material is further crushed, and the particle size is reduced to 10 nanometers to 50 nanometers, and the size distribution is further homogenized, so as to better achieve uniform, complete, and conformal coating.

[0040] In some embodiments, the particle size of the molecular sieve after crushing in step A1 is 100nm to 500nm. Preferably, the particle size of the molecular sieve after crushing in step A1 is 100nm, 200nm, 300nm, 400nm, 500nm. The molecular sieve is crushed to reduce the particle size of the molecular sieve, making it easier to coat the surface of the amorphous carbon, and the coating is tighter and more secure.

[0041] In some embodiments, the thickness of the coating layer in step A2 is 10 nm to 100 nm. Specifically, the thickness of the coating layer in step A2 is 10 nm, 50 nm, 60 nm, or 100 nm.

[0042] In some embodiments, the temperature of the heat treatment in step A3 is 300-600°C, the heating rate is 1-10°C / minute, and the heat treatment time is 1-5 hours. Specifically, the temperature of the heat treatment in step A3 is 300°C, 400°C, 500°C, 600°C, preferably, the heating rate is 1°C / minute, 2°C / minute, 3°C / minute, 4°C / minute, 5°C / minute, 6°C / minute, 7°C / minute, 8°C / minute, 9°C / minute, 10°C / minute, preferably, the heat treatment time is 1 hour, 2 hours, 3 hours, 4 hours. More preferably, the heat treatment temperature is 400-500°C and the heat treatment time is 2-3 hours. Under this condition, the molecular sieve and the amorphous carbon can physically interact with each other to improve the binding force of the molecular sieve and the amorphous carbon. When a sodium-containing molecular sieve is used, the amorphous carbon can achieve a certain degree of chemical pre-sodiumization. The so-called chemical pre-sodiumization refers to the chemical reaction between the sodium in the molecular sieve and the oxygen-containing functional groups (-COOH, -OH, etc.) on the surface of the amorphous carbon to generate -COONa, -ONa, thereby reducing the Na from the positive electrode. + React with these functional groups to improve the first coulombic efficiency and better inhibit the co-intercalation of solvents. In addition, high-temperature heat treatment can also remove the crystallization water contained in the molecular sieve, thereby improving the first coulombic efficiency, capacity and cycle life of amorphous carbon.

[0043] Preferably, the inert atmosphere is one of argon, nitrogen or helium. The reaction is carried out in an inert atmosphere to prevent the molecular sieve or amorphous carbon from reacting with air under heating conditions, thereby affecting the performance of the modified amorphous material.

[0044] A negative electrode sheet comprises the modified amorphous carbon material. The negative electrode sheet of the present invention has good electrochemical performance.

[0045] A sodium ion battery comprises the above-mentioned negative electrode sheet. The sodium ion battery of the invention has few side reactions, high initial coulombic efficiency and long cycle life.

[0046] The modified amorphous carbon material of the present invention has a good structure, few side reactions, low energy consumption for preparation, low cost, short cycle, and is conducive to large-scale production. The modified crystalline carbon material of the present invention contains a molecular sieve on the surface, which plays the role of an artificial SEI, can effectively protect the amorphous carbon, and is conducive to achieving an optimal balance among capacity, coulombic efficiency, and cycle life.

[0047] Example 1

[0048] First, the commercial 4A molecular sieve is sand-milled (the Na / Si molar ratio of the 4A molecular sieve is about 1:1) to a particle size of 200 nanometers. Then, the commercial hard carbon and the sand-milled 4A molecular sieve are mixed evenly at a weight ratio of 100:1. The molecular sieve is uniformly, completely, and conformally coated on the surface of the hard carbon particles by mechanical fusion. Finally, it is heated at 400°C in argon for 3 hours to obtain a surface-modified hard carbon material. The product is analyzed by SEM, and the molecular sieve is uniformly, completely, and conformally coated on the surface of the hard carbon particles. Figure 1 .

[0049] The modified hard carbon material prepared in this embodiment was used as the working electrode, sodium metal as the counter electrode, a glass fiber membrane as the diaphragm, and a NaPF6 propylene carbonate (PC) / ethyl methyl carbonate (EMC) solution as the electrolyte. Constant current charge and discharge tests were performed (current density 30 mA / g, voltage range 0.0052 V ~ 2.0 V). The test results showed that the first charge and discharge capacities of the material were 311 mAh / g and 362 mAh / g, respectively, and the first storage efficiency was 86.0%. The charge and discharge curves are shown in FIG. Figure 2 After 100 cycles, the capacity retention rate is 91%.

[0050] Example 2

[0051] First, the commercial 3A molecular sieve is sand-milled (3A molecular sieve Na / Si molar ratio is about 1:3) to a particle size of 100 nanometers, and then the commercial hard carbon and the sand-milled 3A molecular sieve are mixed uniformly at a weight ratio of 100:1.5, and the molecular sieve is uniformly, completely and conformally coated on the surface of the hard carbon particles by mechanical fusion method, and finally heated at 450°C in argon for 2.5 hours to obtain a surface-modified hard carbon material. The electrochemical test conditions are the same as those in Example 1, and the test results show that the first charge and discharge capacities of the material are 309 mAh / g and 368 mAh / g, respectively, and the first storage efficiency is 83.9%.

[0052] Example 3

[0053] First, the commercial 5A molecular sieve is sand-milled (5A molecular sieve Na / Si molar ratio is about 1:4) to a particle size of 300 nanometers, and then the commercial hard carbon and the sand-milled 5A molecular sieve are mixed uniformly at a weight ratio of 100:2, and the molecular sieve is uniformly, completely and conformally coated on the surface of the hard carbon particles by mechanical fusion method, and finally heated at 500°C for 2 hours in argon to obtain a surface-modified hard carbon material. The electrochemical test conditions are the same as those in Example 1, and the test results show that the first charge and discharge capacities of the material are 298 mAh / g and 359 mAh / g, respectively, and the first storage efficiency is 83.0%.

[0054] Example 4

[0055] First, the commercial TS-1 molecular sieve is sand-milled (Na2O content <0.1wt%) to a particle size of 200 nanometers, and then the commercial soft carbon and the sand-milled Y-type molecular sieve are mixed uniformly at a weight ratio of 100:1, and the molecular sieve is uniformly, completely, and conformally coated on the surface of the soft carbon particles by mechanical fusion, and finally heated at 400°C in argon for 3 hours to obtain a surface-modified soft carbon material. The electrochemical test conditions are the same as those in Example 1, and the test results show that the first charge and discharge capacities of the material are 267mAh / g and 330mAh / g, respectively, and the first storage efficiency is 81.0%.

[0056] Comparative Example 1

[0057] The commercial hard carbon in Example 1 was directly used for electrochemical testing. The test conditions were the same as in Example 1. The test results showed that the first charge and discharge capacities of the material were 291 mAh / g and 386 mAh / g, respectively, and the first storage efficiency was 75.4%. The charge and discharge curves were as follows: Figure 3 After 100 cycles, the capacity retention rate is 67%.

[0058] Comparative Example 2

[0059] The hard carbon modification process is the same as in Example 1, except that no heat treatment is performed after coating. The electrochemical test conditions are the same as in Example 1. The test results show that the first charge and discharge capacities of the material are 296 mAh / g and 377 mAh / g, respectively, and the first storage efficiency is 79.1%. After 100 cycles, the capacity retention rate is 82%.

[0060] Comparative Example 3

[0061] The hard carbon modification process is the same as in Example 1, except that the heat treatment temperature is 200°C. The electrochemical test conditions are the same as in Example 1. The test results show that the first charge and discharge capacities of the material are 298 mAh / g and 367 mAh / g, respectively, and the first storage efficiency is 81.1%. After 100 cycles, the capacity retention rate is 85%.

[0062] By comparing the above examples 1-4 and comparative examples 1-3, it can be seen that the secondary battery prepared by the present invention has higher capacity, higher initial coulombic efficiency, and higher capacity retention rate. Moreover, the initial efficiency of the present invention is as high as 86%, and after 100 charge and discharge cycles, the capacity retention rate is as high as 91%, which has good performance.

[0063] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A method for preparing a modified amorphous carbon material, characterized in that: The steps include: Step A1, providing a molecular sieve, and crushing the molecular sieve, wherein the particle size of the molecular sieve after crushing is 100nm~500nm; Step A2, providing amorphous carbon, uniformly mixing the amorphous carbon and the crushed molecular sieve, and coating the molecular sieve on the surface of the amorphous carbon to form a coating layer to obtain composite particles; Step A3: heat-treating the composite particles under an inert atmosphere to obtain a modified amorphous carbon material, wherein the modified amorphous carbon material has a core-shell structure, wherein the outer shell is a molecular sieve and the inner core is amorphous carbon, and the amorphous carbon includes soft carbon and hard carbon.

2. The method for preparing a modified amorphous carbon material according to claim 1, characterized in that: In the step A3, the inner core accounts for 90% to 99% of the weight of the modified amorphous carbon material, and the outer shell accounts for 1% to 10% of the weight of the amorphous carbon material.

3. The method for preparing a modified amorphous carbon material according to claim 1, characterized in that: The thickness of the coating layer in step A2 is 10nm~100nm.

4. The method for preparing a modified amorphous carbon material according to claim 1, characterized in that: The heat treatment temperature in step A3 is 300-600° C., the heating rate is 1-10° C. / min, and the heat treatment time is 1-5 hours.

5. The method for preparing a modified amorphous carbon material according to claim 1, characterized in that: The inert atmosphere is one of argon, nitrogen or helium.

6. A modified amorphous carbon material, characterized in that: Prepared according to the method for preparing the modified amorphous carbon material according to any one of claims 1 to 5.

7. A negative electrode sheet, characterized in that: Includes the modified amorphous carbon material as described in claim 6.

8. A sodium ion battery, characterized in that: Includes the negative electrode sheet as described in claim 7.