A waste gas purification catalyst and its preparation method and application
By controlling the pore size distribution of the catalyst coating, the problem of unreasonable pore structure in the catalyst coating was solved, the service life and catalytic efficiency of the catalyst were improved, and the diffusion ability of gaseous components was enhanced.
Patent Information
- Application Number
- CN202111233450.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-10-22
AI Technical Summary
The pore structure of the catalytic coating in existing monolithic catalysts is unreasonable, resulting in low diffusion efficiency of gas phase components and affecting the catalytic oxidation reaction effect.
By controlling the particle size ratio of the catalytic performance components and the binder components, the pore size distribution of the catalyst coating can be regulated, thereby improving the coating's adhesion and catalytic performance.
It improves the catalyst's lifespan and catalytic efficiency, enhances the diffusion capacity of gaseous components within the catalyst, and improves the catalytic oxidation reaction effect.
Smart Images

Figure CN115999541B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an exhaust gas purification catalyst, a preparation method of the catalyst and application thereof. Background Art
[0002] Monolithic catalysts are widely used in the purification of mobile and stationary exhaust gases. Such catalysts are usually coated on the surface of a monolithic substrate with catalytically active components to form a catalyst coating with a thickness of tens to tens of microns. Therefore, the properties of the catalyst coating will significantly affect the macroscopic performance of the catalyst.
[0003] Taking the pore structure of the catalyst coating as an example, different pore size distributions have a significant effect on the multi-stage diffusion of gas phase components from the boundary to the inside of the coating and then to the catalytic active sites. Marek et al. demonstrated through experiments and simulations that when there are certain gaps and pores between the particles in the coating, the presence of micron-sized macropores helps increase the diffusion coefficient of gas phase components and promotes the catalytic oxidation reaction of CO. Summary of the invention
[0004] The purpose of the present invention is to provide an exhaust gas purification catalyst in view of the problems of the prior art. The catalyst comprises a catalytic performance component and a binder component, which can simultaneously improve the adhesion of the catalyst coating and increase the service life of the catalyst.
[0005] One aspect of the present invention provides an exhaust gas purification catalyst, comprising: a substrate and a coating located on the substrate, wherein the coating comprises a catalytic performance component and a binder component; in the coating, the ratio V1 / V2 of the pore volume V1 with a pore diameter less than 300 nm to the pore volume V2 with a pore diameter greater than or equal to 300 nm is between 0.1 and 5.
[0006] According to some preferred embodiments of the present invention, V1 / V2 is 0.5-5. In some embodiments, V1 / V2 is 0.5, 0.6, 0.8, 1.0, 1.2, 1.5, 1.8, 2.0, 2.2, 2.5, 2.8, 3.0, 3.5, 3.8, 4.0, 4.5, 4.8, etc.
[0007] According to some embodiments of the present invention, the D50 of the catalytic performance component is between 0.1 μm and 15 μm, preferably between 1 μm and 15 μm. In some embodiments, the D50 of the catalytic performance component is 1 μm, 5 μm, 10 μm, or 15 μm.
[0008] Those skilled in the art know that D50 refers to the particle size at which the cumulative distribution of particles is 50%, also called the median particle size or the median particle size.
[0009] According to some embodiments of the present invention, the catalytic performance component includes one or more of an oxide containing aluminum oxide, a platinum metal, a molecular sieve, and an oxygen storage and release material containing cerium oxide. In some embodiments, the catalytic performance component includes Pt, La, and Al2O3.
[0010] According to some embodiments of the present invention, the binder component contains one or more selected from Al2O3, SiO2, TiO2, transition metal oxides, and rare earth metal oxides.
[0011] According to some embodiments of the present invention, the transition metal oxide is one or more of zirconium oxide, iron oxide, nickel oxide, and cobalt oxide.
[0012] According to some embodiments of the present invention, the rare earth metal oxide is one or more of cerium oxide, lanthanum oxide, neodymium oxide, yttrium oxide, praseodymium oxide and samarium oxide.
[0013] According to some embodiments of the present invention, the binder component accounts for 1%-50% of the coating by mass, preferably 5%-20%. In some embodiments, the binder component accounts for 5%, 10%, 15%, 18%, 20% and the like of the coating by mass.
[0014] According to some embodiments of the present invention, the thickness of the coating is in the range of 10 μm-200 μm.
[0015] According to some embodiments of the present invention, the substrate comprises a honeycomb structure with parallel channels, a corrugated plate structure or a foam structure with interconnected 3D channels. In some preferred embodiments, the substrate is a cordierite honeycomb carrier.
[0016] In the second aspect of the present invention, a method for preparing a waste purification catalyst as described above is provided, which comprises the following steps: S1. preparing a slurry A having a catalytic performance component; S2. dispersing a binder component in the slurry A to obtain a slurry B; S3. coating the slurry B on the surface of a substrate to obtain a catalyst, wherein the ratio of the D50 of the binder component used in step S2 to the D50 of the catalytic performance component used in step S1 is less than or equal to 1:50.
[0017] According to some embodiments of the present invention, the ratio of D50 of the binder component used in step S2 to the D50 of the catalytic performance component used in step S1 is 0.001: 1 to 0.02: 1. In some embodiments, the ratio of D50 of the binder component used in step S2 to the D50 of the catalytic performance component used in step S1 is 0.0012: 1, 0.0024: 1, 0.003: 1, 0.004: 1, 0.005: 1, 0.006: 1, 0.007: 1, 0.009: 1, 0.01: 1, 0.02: 1, etc.
[0018] According to some embodiments of the present invention, the D50 of the binder component used in step S2 is in the range of 0.001 μm-0.2 μm (i.e., 1 nm-200 nm), preferably in the range of 0.01 μm-0.2 μm (i.e., 10 nm-200 nm. In some embodiments, the D50 of the binder component used in step S2 is 10 nm, 20 nm, 30 nm, 50 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, etc.
[0019] According to some embodiments of the present invention, the substrate comprises a honeycomb structure with parallel channels, a corrugated plate structure or a foam structure with interconnected 3D channels. In some preferred embodiments, the substrate is a cordierite honeycomb carrier.
[0020] In a third aspect, the present invention also provides use of the exhaust gas purification catalyst as described above in exhaust gas purification treatment.
[0021] The present invention regulates the influence on the bonding performance of the catalyst coating by controlling the particle size ratio of the binder and the catalytic performance component, and the coating has a specific pore size distribution, thereby improving the performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The pore size distribution of the catalyst coating prepared according to Example 1 is shown.
[0023] Figure 2 The performance comparison of the catalyst prepared in Example 1 and Comparative Example 1 is shown. DETAILED DESCRIPTION
[0024] The present invention will be further described below by way of examples, but are not limited thereto.
[0025] Example 1
[0026] Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by impregnation method was dispersed in water, and the agglomerated powder was ground and dispersed by ball milling, and its D50=9.3μm. Then, a silica sol binder with a particle size of 15.8nm was added, and the amount added was 5% based on the total mass of the coating after calcination. In addition, an organic auxiliary agent polyethylene glycol was added to adjust the stability of the catalyst slurry, and the amount added was 2% based on the total mass of the coating after calcination. The solid content of the slurry was controlled to 27wt%, and then the slurry was coated on a cordierite honeycomb carrier with a pore density of 200 meshes. After drying, it was calcined at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 with a pore size less than 300nm, the pore volume V2 with a pore size greater than or equal to 300nm, and their ratios are shown in Table 1.
[0027] Example 2
[0028] Take the Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=9.3μm. Then add a silica sol binder with a particle size of 27nm, and the amount added is 5% based on the total mass of the coating after calcination. In addition, add an organic auxiliary agent polyethylene glycol to adjust the stability of the catalyst slurry, and the amount added is 2% based on the total mass of the coating after calcination. The solid content of the slurry is controlled to 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 meshes. After drying, it is calcined at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 less than 300nm pore size, the pore volume V2 greater than or equal to 300nm pore size and their ratio are shown in Table 1.
[0029] Example 3
[0030] Take the Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=9.3μm. Then add cerium oxide sol binder with a particle size of 89nm, and the amount added is 5% based on the total mass of the coating after calcination. In addition, organic auxiliary agent polyethylene glycol is added to adjust the stability of the catalyst slurry, and the amount added is 2% based on the total mass of the coating after calcination. The solid content of the slurry is controlled to 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 meshes. After drying, it is calcined at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 less than 300nm pore size, the pore volume V2 greater than or equal to 300nm pore size and their ratio are shown in Table 1.
[0031] Example 4
[0032] Take the Pt / La-Al2O3 catalyst powder prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=9.3μm. Then add cerium oxide-zirconia sol binder with a particle size of 167nm, and the amount added is 5% based on the total mass of the coating after calcination. In addition, add organic auxiliary agent polyethylene glycol to adjust the stability of the catalyst slurry, and the amount added is 2% based on the total mass of the coating after calcination. The solid content of the slurry is controlled to 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 mesh. After drying, it is calcined at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 with a pore size less than 300nm, the pore volume V2 with a pore size greater than or equal to 300nm, and their ratios are shown in Table 1.
[0033] Example 5
[0034] Take the Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=4.2μm. Then add a silica sol binder with a particle size of 15.8nm, and the amount added is 8% based on the total mass of the coating after calcination. In addition, an organic auxiliary agent polyethylene glycol is added to adjust the stability of the catalyst slurry, and the amount added is 2% based on the total mass of the coating after calcination. The solid content of the slurry is controlled to 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 meshes. After drying, it is calcined at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 less than 300nm pore size, the pore volume V2 greater than or equal to 300nm pore size and their ratio are shown in Table 1.
[0035] Example 6
[0036] Take the Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=14.8μm. Then add aluminum sol binder with a particle size of 100nm, and the added amount is 5% based on the total mass of the coating after baking. In addition, add organic additives to adjust the stability of the catalyst slurry, and the added amount is 2% based on the total mass of the coating after baking. The solid content of the slurry is controlled to 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 meshes. After drying, it is baked at 550℃ for 4 hours to obtain a catalyst with a catalytically active coating. The pore volume V1 less than 300nm pore size, the pore volume V2 greater than or equal to 300nm pore size and their ratio are shown in Table 1.
[0037] Comparative Example 1
[0038] Take the Pt / La-Al2O3 catalyst powder (containing 1wt% Pt element) prepared by the impregnation method as in Example 1 and disperse it in water. Grind and disperse the agglomerated powder by ball milling, and its D50=4.1μm. Then add aluminum sol binder with a particle size of 200nm, and the added amount is 5% based on the total mass of the coating after baking. The solid content of the slurry is controlled to be 27wt%, and then the slurry is coated on a cordierite honeycomb carrier with a pore density of 200 mesh. After drying and baking at 550℃ for 4 hours, a catalyst with a catalytically active coating is obtained. The pore volume V1 with a pore size less than 300nm, the pore volume V2 with a pore size greater than or equal to 300nm, and their ratio are shown in Table 1.
[0039] Application Examples
[0040] In the application examples, toluene is used as a typical model compound, and the performance of the catalyst is evaluated by examining the removal efficiency of toluene. The specific gas composition is shown in Table 2.
[0041] The performance of the catalysts prepared in Examples 1-6 and Comparative Example 1 was evaluated. The catalyst was placed in a fixed bed reactor and the gas flow rate was controlled to make the reaction space velocity 20000 h -1 , is the common space velocity in industrial applications. The purification efficiency of the catalyst refers to the purification efficiency of toluene in the gas, which is calculated according to the following formula:
[0042] X=(c tn -c out ) / c tn ×100%
[0043] Among them, X is the purification efficiency, C in is the toluene concentration in the gas before the reaction, ppmv; C out is the toluene concentration in the tail gas after the reaction, ppmv.
[0044] In addition, T in Table 3 90 It refers to the reaction temperature when the purification efficiency reaches 90%. In the present invention, T 90 Refers to the reaction temperature when the toluene purification efficiency reaches 90%.
[0045] Table 1
[0046] <![CDATA[V1(mL / g)]]> <![CDATA[V2(mL / g)]]> <![CDATA[V1 / V2]]> Example 1 0.065 0.097 0.67 Example 2 0.071 0.077 0.92 Example 3 0.086 0.040 2.15 Example 4 0.088 0.037 2.31 Example 5 0.076 0.082 0.93 Example 6 0.058 0.102 0.57 Comparative Example 1 0.091 0.012 7.6
[0047] Table 2
[0048] content Toluene (ppmv) 2000 <![CDATA[H2O(vol%)]]> 5 <![CDATA[O2(vol%)]]> 10 <![CDATA[N2(vol%)]]> Balance gas
[0049] Table 3
[0050] catalyst <![CDATA[GHSV(h -1 )]]> <![CDATA[T 90 (℃)]]> Example 1 20000 186 Example 2 20000 190 Example 3 20000 192 Example 4 20000 200 Example 5 20000 188 Example 6 20000 187 Comparative Example 1 20000 206
[0051] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. An exhaust gas purification catalyst comprising: A substrate and a coating on the substrate, wherein the coating comprises a catalytic performance component and a binder component; In the coating, the ratio V1 / V2 of the pore volume V1 with a pore diameter less than 300 nm to the pore volume V2 with a pore diameter greater than or equal to 300 nm is in the range of 0.1-5; The catalytic performance component includes one or more of an oxide containing aluminum oxide, a platinum metal, a molecular sieve, and an oxygen storage and release material containing cerium oxide; The D50 of the catalytic performance component is in the range of 0.1 μm to 15 μm.
2. The catalyst according to claim 1, characterized in that V1 / V2 is in the range of 0.5-5.
3. The catalyst according to claim 1, characterized in that The D50 of the catalytic performance component is in the range of 1 μm-15 μm.
4. The catalyst according to any one of claims 1 to 3, characterized in that The binder component includes one or more of Al2O3, SiO2, TiO2, transition metal oxides, and rare earth metal oxides.
5. The catalyst according to claim 4, characterized in that The transition metal oxide is one or more of zirconium oxide, iron oxide, nickel oxide, and cobalt oxide, and the rare earth metal oxide is one or more of cerium oxide, lanthanum oxide, neodymium oxide, yttrium oxide, praseodymium oxide, and samarium oxide.
6. The catalyst according to any one of claims 1 to 3, characterized in that The mass percentage of the binder component in the coating is in the range of 1%-50%.
7. The catalyst according to claim 6, characterized in that The mass percentage of the binder component in the coating is in the range of 5%-20%.
8. The catalyst according to any one of claims 1 to 3, characterized in that The substrate comprises a honeycomb structure with parallel pores, a corrugated plate structure or a foam structure with interconnected 3D pores.
9. A method for preparing the catalyst according to any one of claims 1 to 8, comprising the steps of: S1. Preparing a slurry A having a catalytic component; S2. dispersing the binder component in slurry A to obtain slurry B; S3. Coating slurry B on the surface of the substrate to obtain a catalyst, in, The ratio of the average particle size D50 of the binder component used in step S2 to the average particle size D50 of the catalytic performance component used in step S1 is less than or equal to 0.02:
1.
10. The preparation method according to claim 9, characterized in that: The ratio of the average particle size D50 of the binder component used in step S2 to the average particle size D50 of the catalytic performance component used in step S1 is 0.001:1 to 0.02:
1.
11. The preparation method according to claim 9 or 10, characterized in that: The D50 of the binder component used in step S2 is in the range of 0.001 μm to 0.2 μm.
12. Use of the exhaust gas purification catalyst according to any one of claims 1 to 8 or the exhaust gas purification catalyst prepared by the preparation method according to any one of claims 9 to 11 in exhaust gas purification treatment.