Polymer solid electrolyte, method for producing the same, and electrochemical device

By using polymer solid electrolytes in magnesium battery electrochemical devices, including Mg polymer salts and anionic polymers, the problems of flexibility and low ion conductivity of magnesium battery solid electrolytes are solved, and structural maintenance and high ion conductivity are achieved. Improved conductivity.

CN116018360BActive Publication Date: 2024-10-29MURATA MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180053332.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-27
Publication Date
2024-10-29
Estimated Expiration
2041-04-27

AI Technical Summary

Technical Problem

The solid electrolyte of existing magnesium batteries has low flexibility, brittleness and low ionic conductivity, making it difficult to maintain the structure and improve ionic conductivity under stress conditions.

Method used

A polymer solid electrolyte is used, including Mg polymer salt. The Mg polymer salt contains an anionic polymer containing Mg2+ and anionic functional groups and coordination functional groups. The Mg polymer salt is generated through the ion exchange reaction of the Li polymer salt to increase Mg. Ionic conductivity.

Benefits of technology

An electrochemical device with excellent structural maintenance and high ion conductivity has been realized. The Mg polymer salt can recover its shape under stress conditions, and the Mg ion conductivity is significantly improved, solving the flexibility and conductivity problems of solid electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116018360B_ABST
    Figure CN116018360B_ABST
Patent Text Reader

Abstract

A polymer solid electrolyte is a polymer solid electrolyte for an electrochemical device having a magnesium electrode as a negative electrode, comprising a Mg polymer salt, wherein the Mg polymer salt comprises Mg 2+ and an anionic polymer having an anionic functional group and a coordinating functional group, wherein the polymer solid electrolyte has Mg ion conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer solid electrolyte, a method for producing the same and an electrochemical device. Background Art

[0002] Electrochemical devices include capacitors, air batteries, fuel cells, and secondary batteries, and are used in various applications. Electrochemical devices include a positive electrode and a negative electrode, and have a solid electrolyte that is responsible for ion transport between the positive electrode and the negative electrode.

[0003] For example, as an electrode of an electrochemical device represented by a magnesium battery, an electrode composed of magnesium or at least an electrode containing magnesium is provided (hereinafter, such an electrode is simply referred to as a "magnesium electrode", and an electrochemical device using a magnesium electrode is also referred to as an "electrochemical device of a magnesium electrode system"). Magnesium is abundant in resources and very cheap compared to lithium. In addition, the amount of electricity per unit volume that can be taken out by magnesium through redox reactions is generally large, and the safety when used in electrochemical devices is also high. Therefore, magnesium batteries have attracted attention as the next generation of secondary batteries to replace lithium-ion batteries.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: U.S. Patent Publication No. US2018 / 0159170A1

[0007] Patent document 2: U.S. Patent Publication No. US2018 / 0102567A1. Summary of the invention

[0008] Technical problem to be solved by the invention

[0009] As a solid electrolyte for magnesium batteries, it is proposed to use inorganic substances. For example, in Patent Document 1, a solid electrolyte having the general formula Mg x M y SiO z (wherein, in the general formula, M is at least one selected from the group consisting of Ti, Zr, Hf, Ca, Sr and Ba, 0<x<2, 0<y<2 and 3<z<6) an inorganic substance having a composition. In addition, in Patent Document 2, a general formula of Mg is used. x SiO y N z (wherein, in the general formula, 1<x<2, 3<y<5, and 0≤z<1) is an inorganic substance having a composition represented by:

[0010] Since inorganic materials have low flexibility, when used as solid electrolytes, they have the following disadvantages: when stress is applied to the solid electrolyte or when stress is generated in the solid electrolyte, the solid electrolyte is easily broken and difficult to recover to its original shape. In addition, the ion conductivity of the solid electrolyte composed of inorganic materials is extremely low at 10 at 500°C. -9 ~10 - 7 S / cm order of magnitude.

[0011] The present invention has been made in view of such problems. That is, a main object of the present invention is to provide a solid electrolyte having excellent structural retention and being useful for realizing an electrochemical device having higher ion conductivity than before.

[0012] Solutions for solving technical problems

[0013] The inventors of the present application have attempted to solve the above-mentioned problems by addressing the problem in a new direction instead of addressing the problem in the extension of the prior art. As a result, they have completed the invention of a solid electrolyte that achieves the above-mentioned main purpose.

[0014] The present invention provides a polymer solid electrolyte for an electrochemical device having a magnesium electrode as a negative electrode, wherein the polymer solid electrolyte comprises a Mg polymer salt, wherein the Mg polymer salt comprises Mg 2+ and an anionic polymer having an anionic functional group and a coordinating functional group, wherein the polymer solid electrolyte has Mg ion conductivity.

[0015] In addition, the present invention provides a method for producing a polymer solid electrolyte having Mg ion conductivity, the method comprising the following steps: dissolving a Li polymer salt represented by the general formula (4) in a linear ether solution of a Mg salt, adding a linear ether to precipitate a Mg polymer salt represented by the general formula (5),

[0016] [Chemistry 1]

[0017]

[0018] [In the general formula (4), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same as or different from each other.]

[0019] [Chemistry 2]

[0020]

[0021] [In the general formula (5), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same or different from each other.]

[0022] Effects of the Invention

[0023] In the polymer solid electrolyte of the present invention, an electrochemical device having excellent structural maintenance and high ion conductivity can be provided. In other words, in the electrochemical device of the magnesium electrode system using the polymer solid electrolyte of the present invention, the polymer solid electrolyte comprises a Mg polymer salt, and the Mg polymer salt comprises Mg 2+ and an anionic polymer having an anionic functional group and a coordinating functional group. Due to such a structure, the polymer solid electrolyte has high ion conductivity (Mg ion conductivity).

[0024] The electrolyte of the electrochemical device of the magnesium electrode system of the present invention is composed of a Mg polymer salt. Therefore, even when stress is applied to the solid electrolyte or when stress is generated in the solid electrolyte, the Mg polymer salt has high flexibility and can be restored to its original shape. Due to the composition of the above-mentioned polymer solid electrolyte, the structure maintenance is excellent.

[0025] In addition, in the method for producing a polymer solid electrolyte of the present invention, a polymer solid electrolyte is produced that leads to an electrochemical device having excellent structural maintenance and high ion conductivity. The method for producing a polymer solid electrolyte dissolves a Li polymer salt in a linear ether solution of a Mg salt and adds a linear ether to precipitate the Mg polymer salt. In other words, the Li polymer salt is converted to Li by an ion exchange reaction. + Replaced by Mg 2+ , and precipitate to obtain a Mg polymer salt. Therefore, in the obtained Mg polymer salt, the Mg ion concentration is relatively high. Further, the anionic polymer has a structure represented by the general formula (5), especially with Mg 2+ An ionic bond of appropriate strength is formed, and thus, the Mg polymer salt can contribute to high ion conductivity.

[0026] In addition, the effects described in this specification are merely illustrative and not limiting, and additional effects may also occur. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a conceptual diagram of a magnesium electrode-based electrochemical device (particularly a battery) according to one embodiment of the present invention.

[0028] Figure 2This is a schematic cross-sectional view of a magnesium secondary battery (cylindrical magnesium secondary battery) provided as one embodiment of the present invention.

[0029] Figure 3 This is a schematic perspective view of a magnesium secondary battery (a flat-plate laminated film type magnesium secondary battery) provided as one embodiment of the present invention.

[0030] Figure 4 is a schematic cross-sectional view of an electrochemical device provided as a capacitor in one embodiment of the present invention.

[0031] Figure 5 is a schematic cross-sectional view of an electrochemical device provided as an air battery in one embodiment of the present invention.

[0032] Figure 6 This is a block diagram showing an example of a circuit configuration when a magnesium secondary battery provided as one embodiment of the present invention is applied to a battery pack.

[0033] Figure 7 A. Figure 7 B and Figure 7 C is a block diagram showing the configurations of an electric vehicle, a power storage system, and an electric power tool, respectively, to which a magnesium secondary battery is applied as one embodiment of the present invention.

[0034] Figure 8 This is a development diagram schematically showing a battery produced in [Example] of this specification.

[0035] Fig. 9 This is a graph (NMR spectrum) showing the results of "Identification Evaluation" in [Examples] of this specification.

[0036] Fig.10 This is a graph showing the results of “Evaluation of ion conductivity” in [Examples] of this specification (particularly, a graph showing the relationship between ion conductivity and temperature). DETAILED DESCRIPTION

[0037] Hereinafter, the "polymer solid electrolyte for electrochemical devices (hereinafter, the polymer solid electrolyte will also be referred to as a solid electrolyte) and its manufacturing method" and the "electrochemical device" of the present invention are described in detail. The description will be made with reference to the drawings as needed, but the contents of the drawings are only schematically and illustratively shown for the purpose of understanding the present invention, and the appearance and dimensional ratios may be different from the actual objects. In addition, the various numerical ranges mentioned in this specification are intended to also include the lower limit and the upper limit values ​​themselves. In other words, for example, if a numerical range such as 1 to 10 is taken as an example, it can be understood as including the lower limit value "1" and also including the upper limit value "10" unless otherwise specified.

[0038] In the present invention, "electrochemical device" refers to a device that can extract energy by electrochemical reaction in a broad sense. In a narrow sense, "electrochemical device" refers to a device that has a pair of electrodes and an electrolyte, and is charged and discharged with the movement of ions. Although it is just an example, as electrochemical devices, capacitors, air batteries, fuel cells, etc. can also be cited in addition to secondary batteries.

[0039] [Solid electrolytes for electrochemical devices]

[0040] The solid electrolyte of the present invention is used for an electrochemical device. In other words, the solid electrolyte described in this specification corresponds to an electrolyte used for a device that can extract energy by utilizing an electrochemical reaction.

[0041] The solid electrolyte of the present invention is a solid electrolyte for an electrochemical device having a magnesium electrode as its main premise. In particular, it is a solid electrolyte for an electrochemical device having a magnesium electrode as a negative electrode. Therefore, the solid electrolyte of the present invention can also be said to be a solid electrolyte for an electrochemical device of a magnesium electrode system (hereinafter, also simply referred to as a "magnesium electrode system solid electrolyte").

[0042] Although it will be mentioned below, such an electrochemical device preferably has a magnesium electrode as the negative electrode and a sulfur electrode as the positive electrode. In other words, in a preferred embodiment, the solid electrolyte of the present invention is a solid electrolyte for a magnesium (Mg)-sulfur (S) electrode.

[0043] Here, the "magnesium electrode" used in this specification refers to an electrode having magnesium (Mg) as an active component (i.e., an active material) in a broad sense. In a narrow sense, the "magnesium electrode" refers to an electrode composed of magnesium, for example, an electrode composed of magnesium metal or a magnesium alloy, and in particular, a negative electrode of such magnesium. In addition, the above-mentioned magnesium electrode may also contain components other than magnesium metal or magnesium alloy, but in a preferred embodiment, it is an electrode composed of a metal body of magnesium (for example, an electrode composed of a single body of magnesium metal with a purity of 90% or more, preferably a purity of 95% or more, and more preferably a purity of 98% or more).

[0044] In addition, the "sulfur electrode" used in this specification refers to an electrode having sulfur (S) as an active component (i.e., an active material) in a broad sense. In a narrow sense, the "sulfur electrode" refers to an electrode composed of at least sulfur, for example, an electrode composed of sulfur (S) such as S8 and / or polymeric sulfur, and particularly refers to such a sulfur positive electrode. In addition, the sulfur electrode may also contain components other than sulfur, for example, it may also contain a conductive auxiliary agent and a binder. Although it is only an example, the sulfur content in the sulfur electrode may be 5% by mass or more and 95% by mass or less, for example, 70% by mass or more and 90% by mass or less based on the entire electrode (in addition, in a certain example, the sulfur content in the sulfur electrode may be 5% by mass to 20% by mass or 5% by mass to 15% by mass, etc.).

[0045] The solid electrolyte of the magnesium electrode system according to the present invention has Mg ion conductivity. The ion conductivity of the solid electrolyte is, for example, 10 -5 The ion conductivity is a value of the order of 10 S / cm. The method for determining the ion conductivity is described in detail in the examples. In conventional solid electrolytes composed of inorganic substances, the Mg ion conductivity is 10 -9 ~10 -7 For example, in Patent Documents 1 and 2, the value of S / cm at 500°C is 1.1×10 -9 ~about 3.6×10 -7 S / cm.

[0046] The solid electrolyte includes a Mg polymer salt. Since the solid electrolyte includes a Mg polymer salt, even when stress is applied to the solid electrolyte or stress is generated in the solid electrolyte, the Mg polymer salt can return to its original shape due to its high flexibility. Therefore, the solid electrolyte has excellent structural maintenance.

[0047] In addition, the solid electrolyte is solid, not liquid (electrolyte). In the solid electrolyte, no organic solvent is contained, so there is no worry about the electrolyte leaking from the electrical device, etc., and the safety and operability are excellent. In addition, the solid electrolyte does not contain an organic solvent, so it has excellent thermal stability. In addition, the solid electrolyte does not contain an organic solvent as a dispersant because the coordination functional group of the anionic polymer will make Mg 2+ Dispersed in solid electrolyte.

[0048] In addition, the Mg polymer salt contains Mg 2+ and anionic polymers having anionic functional groups and coordinating functional groups. Due to such a structure of the solid electrolyte, it has high ionic conductivity. Although not bound by a specific theory, the reason is presumed to be as follows. The coordinating functional groups make Mg2+ Dispersed in the solid electrolyte. The anionic polymer has a certain degree of intramolecular mobility in the solid electrolyte, for example, the molecular chain of the anionic polymer having anionic functional groups moves. The anionic functional groups (for example, monovalent negatively charged functional groups) are in contact with the counter ion Mg. 2+ The electrostatic attraction between them causes the movement of anionic functional groups. 2+ In this way, the anionic polymer efficiently transports Mg as a carrier in the solid electrolyte. 2+ , therefore, Mg 2+ The ion transfer number is increased and the Mg ion conductivity of the solid electrolyte is high.

[0049] The Mg polymer salt may be, for example, a triblock copolymer (ABA type triblock copolymer) represented by the general formula (1).

[0050] [Chemistry 3]

[0051] (A)-(B)-(A) (1)

[0052] [In the general formula (1), (A) represents a block having an anionic functional group, and (B) represents a block having a coordinating functional group. The two (A)s may be the same or different from each other.]

[0053] In the general formula (1), (A) may be a block represented by the general formula (2).

[0054] [Chemistry 4]

[0055]

[0056] [In the general formula (2), Af represents an anionic functional group, m represents an integer of 3 to 40, and p represents an integer of 1 to 10.]

[0057] In the general formula (2), from the viewpoint of further improving the Mg ion conductivity, it is preferred that p represents 3 and m represents 20 to 40.

[0058] In the general formula (2), as the alkylene group -(CH2) p -Specific examples include methylene, ethylene, n-propylene, n-butylene, n-pentylene, n-hexylene, n-heptylene, n-octylene, n-nonylene and n-decylene. The m alkylene groups in the m repeating units represented by the general formula (2) may be the same as or different from each other. Among these alkylene groups, n-propylene is preferred from the viewpoint of improving Mg ion conductivity.

[0059] The valence of the anionic functional group may also be monovalent or polyvalent (e.g., divalent, etc.). The anionic functional group is preferably a monovalent anionic functional group. In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, it is speculated that the reason is as follows. The anionic functional group is in the presence of Mg as a counter ion in the solid electrolyte. 2+ Here, compared with the anionic functional groups with a valence of more than 2, the anionic functional groups with a valence of 1 or 2 have a smaller valence, so they are more likely to bind to Mg. 2+ Therefore, the monovalent anionic functional group forms a relatively weak ionic bond with Mg. 2+ The ionic bonds of appropriate strength are formed between them, which inhibits the Mg 2+ Therefore, it is believed that Mg 2+ The ion migration number is increased and the Mg ion conductivity is further improved.

[0060] The anionic functional group is more preferably a perfluoroalkylsulfonamide group (C k F 2k+1 -SO2-N - -SO2-; wherein k represents an integer of 1 to 10. ) and -SO3 - The group is more preferably a perfluoroalkylsulfonamide group, and particularly preferably a trifluoromethylsulfonamide group (CF3-SO2-N - -SO2- group). The m anionic functional groups in the m repeating units represented by the general formula (2) may be the same as or different from each other.

[0061] For perfluoroalkylsulfonamide and -SO3 - Therefore, if the anionic functional group is a perfluoroalkylsulfonamide group or -SO3 - The anionic functional group is in the presence of Mg 2+ The ionic bonds of appropriate strength are formed between Mg 2+ The electrostatic attraction between the anionic functional groups prevents Mg 2+ The degree of strong binding to the anionic functional groups is moderate. In this way, the Mg 2+ Therefore, Mg 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0062] The anionic polymer preferably has an anionic functional group in the side chain as shown in the general formula (2). In this case, the Mg ion conductivity of the solid electrolyte is further improved. Although not bound by a specific theory, the reason is presumed to be as follows. The side chain of the anionic polymer has a higher degree of freedom of movement than the main chain, for example, the side chain moves in the solid electrolyte in a manner that allows the side chain to swing. 2+ There is electrostatic attraction between them, so along with the movement of the side chain of the anionic polymer, Mg 2+ Therefore, if the anionic polymer has an anionic functional group in the side chain, Mg 2+ The ion transfer number is further improved, and it is considered that the Mg ion conductivity of the solid electrolyte is further improved.

[0063] In the general formula (1), (B) may be a block represented by the general formula (3).

[0064] [Chemistry 5]

[0065]

[0066] [In the general formula (3), n represents an integer of 150 to 850, and q represents an integer of 1 to 10.]

[0067] In the general formula (3), q preferably represents 2 from the viewpoint of further improving Mg ion conductivity.

[0068] The block represented by the general formula (3) is a poly(alkylene oxide) in which a plurality of alkyleneoxy structural units are bonded in a linear chain. Here, the "alkyleneoxy structural unit" refers to a molecular structural unit in which an alkylene group is bonded to an oxygen atom (-(CH2) q -O-) (q in the molecular structural unit has the same meaning as q in the general formula (3).).

[0069] The poly(alkylene oxide) represented by the general formula (3) is, for example, a poly(alkylene oxide) having 1 to 10 carbon atoms. Specific examples of the poly(alkylene oxide) include poly(formaldehyde), poly(ethylene oxide), poly(n-propylene oxide), poly(n-butylene oxide), poly(n-pentyl oxide), poly(n-hexyl oxide), poly(n-heptyl oxide), poly(n-octyl oxide), poly(n-nonyl oxide) and poly(n-decyl oxide). Among these poly(alkylene oxides), poly(ethylene oxide) is preferred from the viewpoint of further improving Mg ion conductivity.

[0070] The multiple alkylene oxide structural units of the block represented by the general formula (3) are, for example, multiple alkylene oxide structural units having 1 to 10 carbon atoms. Specific examples of the alkylene oxide in the structural unit include methylene oxide, ethylene oxide, n-propylene oxide, n-butylene oxide, n-pentylene oxide, n-hexylene oxide, n-heptylene oxide, n-octylene oxide, n-nonylene oxide and n-decylene oxide. Among these alkylene oxides, ethylene oxide is preferred from the viewpoint of further improving Mg ion conductivity.

[0071] The anionic polymer preferably has a coordinating functional group in the main chain, as represented by the general formula (3). In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, the reason is presumed to be as follows. The coordinating functional group has a relatively flexible structure, so if the anionic polymer has a coordinating functional group in the main chain, the freedom of movement of the anionic polymer is improved. Electrostatic attraction acts on the anionic functional group and Mg 2+ Therefore, along with the movement of the main chain of the anionic polymer, Mg 2+ Therefore, if the anionic polymer has a coordinating functional group in the main chain, Mg 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0072] The coordinating functional group is preferably a poly(alkylene oxide), and more preferably a poly(ethylene oxide) (a poly(alkylene oxide) when q represents 2 in the general formula (3)). In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, it is speculated that the reason is as follows. Poly(ethylene oxide) has a relatively flexible structure, so if the anionic polymer has poly(ethylene oxide) as a coordinating functional group, the freedom of movement of the anionic polymer is improved. In addition, the lone pair of electrons of the oxygen atom of the polyalkylene oxide is easily coordinated to the Mg ion. 2+ Therefore, the Mg in the solid electrolyte 2+ The dispersibility of Mg is further improved. 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0073] The Mg polymer salt represented by the general formula (1) may be, for example, a Mg polymer salt represented by the general formula (5) (hereinafter, the Mg polymer salt represented by the general formula (5) is also referred to as "Mg polymer salt (5)").

[0074] [Chemistry 6]

[0075]

[0076] [In the general formula (5), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same as or different from each other.]

[0077] In addition, m, p, Af, n, and q in the general formula (5) are synonymous with m, p, Af in the general formula (2) and n and q in the general formula (3), respectively. In addition, as T in the general formula (5), for example, C6H5C(=S)S- can be cited. In addition, Af in the general formula (5) represents a monovalent anionic functional group.

[0078] The number average molecular weight Mn of the Mg polymer salt is, for example, 12,000 to 60,000. The method for measuring the number average molecular weight of the Mg polymer salt will be described in detail with reference to Examples.

[0079] Examples of the Mg polymer salt (5) include a Mg polymer salt represented by the general formula (5-2) (hereinafter also referred to as “Mg polymer salt (5-2)”).

[0080] [Chemistry 7]

[0081]

[0082] [In the general formula (5-2), m represents an integer of 3 to 40, and n represents an integer of 150 to 850.]

[0083] The solid electrolyte may also be composed of a Mg polymer salt.

[0084] The magnesium electrode system solid electrolyte involved in the present invention is preferably used for an electrochemical device having a magnesium electrode as a negative electrode, but it is more preferable when the device has a sulfur electrode as a positive electrode. In other words, when the solid electrolyte of the present invention is a solid electrolyte for an electrochemical device having a magnesium electrode as a negative electrode, it is preferred that the positive electrode of the electrochemical device is a sulfur electrode. Hereinafter, an electrochemical device having such a magnesium electrode-sulfur electrode pair is also referred to as a "magnesium-sulfur electrode system electrochemical device".

[0085] [Method for producing solid electrolyte]

[0086] As an example of the method for producing the solid electrolyte of the present invention, a method for synthesizing a Mg polymer salt (5) is described. The method for synthesizing a Mg polymer salt (5) comprises a Li polymer salt synthesis step and an ion exchange step. That is, the Mg polymer salt (5) is synthesized according to reactions (R-1) to (R-2) or by a method according to the reaction scheme shown below.

[0087] [Chemistry 8]

[0088]

[0089] (Li polymer salt synthesis step: reaction (R-1))

[0090] In the Li polymer salt synthesis step, a PAO macrochain transfer agent represented by the general formula (6) (hereinafter also referred to as PAO macrochain transfer agent (6)) and a Li salt of a methacrylic acid derivative represented by the general formula (7) (hereinafter also referred to as Li salt (7)) are subjected to a reversible addition-fragmentation chain polymerization reaction (RAFT reaction: reaction (R-1)) in the presence of a polymerization initiator to synthesize a Li polymer salt represented by the general formula (4) (hereinafter also referred to as Li polymer salt (4)).

[0091] In the reaction (R-1), q and n in the general formula (6), p and Af in the general formula (7) are synonymous with q, n, p and Af in the general formula (5), respectively. m, n, p, q and Af in the general formula (4) are synonymous with m, n, p, q and Af in the general formula (5), respectively. In the general formula (5) in the above reaction scheme, Af represents a monovalent anionic functional group.

[0092] Examples of the polymerization initiator include azo-based polymerization initiators (more specifically, 2,2′-azobis(2-aminopropane) hydrochloride (AIBA)). The polymerization initiator can be added in an amount of, for example, 0.1 to 0.4 mol per 1 mol of the PAO macrochain transfer agent.

[0093] In reaction (R-1), for example, m moles of Li salt (7) are reacted with 1 mole of PAO macrochain transfer agent to obtain 1 mole of Li polymer salt (4). In reaction (R-1), the reaction temperature is preferably 40° C. to 80° C. The reaction time is preferably 8 hours to 15 hours.

[0094] Alternatively, the PAO macrochain transfer agent (6) and the Li salt (7) as starting compounds in the reaction (R-1) can also be prepared by synthesis.

[0095] (Ion exchange step: reaction (R-2))

[0096] In the ion exchange step, the Li polymer salt (4) is subjected to an ion exchange reaction to obtain a Mg polymer salt (5). The Li polymer salt (4) is dissolved in a linear ether solution of a Mg salt (Mg electrolyte). Examples of Mg salts include magnesium chloride (MgCl2), Mg salts of perfluoroalkylsulfonyl imide (more specifically, Mg salts of trifluoromethylsulfonyl imide (magnesium bistrifluoromethanesulfonyl imide: Mg(TFSI)2)) and mixtures thereof. The concentration of the Mg salt is, for example, 0.5 to 3 M (moL / L). From the viewpoint of increasing the yield of the Mg polymer salt (5), the volume of the Mg solution is sufficient to convert the Li + Replaced by Mg 2+ The volume of the reaction mixture is preferably the smallest possible volume required to dissolve the Li polymer salt (4), and more preferably the smallest volume required to dissolve the Li polymer salt (4). Next, a linear ether is added to the obtained Li polymer salt (4) solution to precipitate the Mg polymer salt (5). In addition, the reaction (R-2) can be carried out under an inert gas (e.g., argon) atmosphere.

[0097] The linear ether as the solvent is represented by, for example, the general formula (8).

[0098] [Chemistry 9]

[0099]

[0100] [In the general formula (8), R' and R" each independently represent a hydrocarbon group having 1 to 10 carbon atoms, and n' represents an integer of 1 to 10.]

[0101] The straight-chain ether represented by the general formula (8) has an ethyleneoxy structural unit. In the straight-chain ether having an ethyleneoxy structural unit, in the general formula (8), R' and R" may also be independently an aliphatic hydrocarbon group of 1 or more and 10 or less. In addition, in the straight-chain ether having such an ethyleneoxy structural unit, n' in the general formula (8) may also be an integer of 2 or more and 4 or less, and therefore, the straight-chain ether may also be an ether having 2 or more and 4 or less ethyleneoxy structural units. In addition, in the straight-chain ether having an "ethyleneoxy structural unit", in the general formula (8), R' and R" may also be independently a lower alkyl group having 1 or more and 4 or less carbon atoms. In addition, in the straight-chain ether solvent having an "ethyleneoxy structural unit", in the above general formula, R' and R" may also be mutually identical alkyl groups.

[0102] Although it is just an example, the linear ether having an "ethyleneoxy structural unit" may be at least one selected from the group consisting of ethylene glycol dimethyl ether (dimethoxyethane), diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, pentaethylene glycol dimethyl ether, hexaethylene glycol dimethyl ether and polyethylene glycol dimethyl ether. Among them, dimethoxyethane is preferred.

[0103] Conventionally, there is a problem that the Mg polymer salt (5) cannot be obtained efficiently. For example, in a method in which the Li polymer salt (4) is simply dissolved in a Mg salt solution and the solvent is removed, the Li + It is more difficult because, in addition to the target Mg polymer salt (5), it also contains Li polymer salt (4), and it is impossible to precipitate and recover only Mg polymer salt (5). As a result of careful research conducted by the inventors of the present invention, it was found that the solubility of Li polymer salt (4) in an electrolyte containing glyme solvent varies greatly depending on the electrolyte concentration. Based on this technical insight, the inventors of the present invention have derived that the solubility of Li polymer salt (4) in an electrolyte containing glyme solvent (electrolyte concentration dependence of solubility) can be relatively easily adjusted by the electrolyte concentration in the electrolyte. In addition, the inventors predict that the target Mg polymer salt (5) also shows the electrolyte concentration dependence of solubility. In addition, based on the electrostatic interaction and dissolution between metal ions and anionic polymers, the inventors of the present invention focus on the electrolyte concentration dependence relative to L + The selective ion exchange and coordination of Mg 2+ , deriving the use of Mg salt as the electrolyte. Further, the inventors of the present invention found that: 2+ When the Li polymer salt (4) is coordinated to the anionic polymer, if a glyme solvent is added, the Mg polymer salt (5) can be efficiently precipitated. Based on the above technical insights, the inventors of the present invention have conducted further research and found that by "dissolving the Li polymer salt (4) in a glyme solution of the Mg salt and then adding a glyme solvent", the dissolution of the Li polymer salt (4) and the precipitation of the Mg polymer salt (5) can be simultaneously satisfied, thereby efficiently obtaining the Mg polymer salt (5).

[0104] In addition to the above reaction, necessary steps (e.g., processing steps and purification steps) may also be included. The processing step includes, for example, hot pressing the obtained polymer salt (5) to form a sheet and cutting it, and processing the obtained polymer salt (5) into a predetermined shape. As the purification step, for example, known methods (more specifically, filtration, chromatography, dialysis or crystallization) can be cited.

[0105] [Electrochemical device of the present invention]

[0106] Next, the electrochemical device of the present invention is described. Such an electrochemical device comprises a negative electrode and a positive electrode, and a magnesium electrode is provided as the negative electrode. Such an electrochemical device is characterized in that its solid electrolyte is composed of at least the above-mentioned solid electrolyte.

[0107] In other words, the solid electrolyte of the electrochemical device of the present invention comprises at least a Mg polymer salt, and such a Mg polymer salt comprises Mg 2+ and anionic polymers having anionic functional groups and coordinating functional groups.

[0108] The Mg polymer salt may be, for example, a triblock copolymer (ABA type triblock copolymer) represented by the general formula (1).

[0109] [Chemistry 10]

[0110] (A)-(B)-(A) (1)

[0111] [In the general formula (1), (A) represents a block having an anionic functional group, and (B) represents a block having a coordinating functional group. The two (A)s may be the same or different from each other.]

[0112] In the general formula (1), (A) may be a block represented by the general formula (2).

[0113] [Chemistry 11]

[0114]

[0115] [In the general formula (2), Af represents an anionic functional group, m represents an integer of 3 to 40, and p represents an integer of 1 to 10.]

[0116] In the general formula (2), from the viewpoint of further improving the Mg ion conductivity, it is preferred that p represents 3 and m represents 20 to 40.

[0117] In the general formula (2), as the alkylene group -(CH2) p -Specific examples include methylene, ethylene, n-propylene, n-butylene, n-pentylene, n-hexylene, n-heptylene, n-octylene, n-nonylene and n-decylene. The m alkylene groups in the m repeating units represented by the general formula (2) may be the same as or different from each other. Among these alkylene groups, n-propylene is preferred from the viewpoint of improving Mg ion conductivity.

[0118] The valence of the anionic functional group may also be monovalent or polyvalent (e.g., divalent, etc.). The anionic functional group is preferably a monovalent anionic functional group. In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, it is speculated that the reason is as follows. The anionic functional group is in the presence of Mg as a counter ion in the solid electrolyte. 2+ Here, compared with the anionic functional groups with a valence of more than two, the valence of the monovalent anionic functional groups is smaller, so when they are combined with Mg 2+ Therefore, the monovalent anionic functional group forms a relatively weak ionic bond with Mg. 2+ The ionic bonds of appropriate strength are formed between them, which inhibits the Mg 2+ Therefore, Mg 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0119] The anionic functional group is more preferably a perfluoroalkylsulfonamide group (C k F 2k+1 -SO2-N - -SO2-; wherein k represents an integer of 1 to 10. ) and -SO3 - A group, more preferably a perfluoroalkylsulfonamide group, and particularly preferably a trifluoromethylsulfonamide group (CF3-SO2-N - -SO2- group). The m anionic functional groups in the m repeating units represented by the general formula (2) may be the same as or different from each other.

[0120] For perfluoroalkylsulfonamide and -SO3 - Therefore, if the anionic functional group is a perfluoroalkylsulfonamide group or -SO3 - The anionic functional group is in the presence of Mg 2+ The ionic bonds of appropriate strength are formed between Mg 2+ The electrostatic attraction between the anionic functional groups prevents Mg 2+ The degree of strong binding to the anionic functional groups is moderate. In this way, the Mg 2+ Therefore, Mg 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0121] The anionic polymer preferably has an anionic functional group in the side chain as shown in the general formula (2). In this case, the Mg ion conductivity of the solid electrolyte is further improved. Although not bound by a specific theory, the reason is presumed to be as follows. The side chain of the anionic polymer has a higher degree of freedom of movement than the main chain, for example, the side chain moves in the solid electrolyte in a manner that allows the side chain to swing. 2+ There is electrostatic attraction between them, so along with the movement of the side chain of the anionic polymer, Mg 2+ Therefore, if the anionic polymer has an anionic functional group in the side chain, Mg 2+ The ion transfer number is further improved, and it is considered that the Mg ion conductivity of the solid electrolyte is further improved.

[0122] In the general formula (1), (B) may be a block represented by the general formula (3).

[0123] [Chemistry 12]

[0124]

[0125] [In the general formula (3), n represents an integer of 150 to 850, and q represents an integer of 1 to 10.]

[0126] In the general formula (3), q preferably represents 2 from the viewpoint of further improving Mg ion conductivity.

[0127] The block represented by the general formula (3) is a poly(alkylene oxide) in which a plurality of alkyleneoxy structural units are bonded in a linear chain. Here, the "alkyleneoxy structural unit" refers to a molecular structural unit in which an alkylene group is bonded to an oxygen atom (-(CH2) q -O-) (q in the molecular structural unit has the same meaning as q in the general formula (3).).

[0128] The poly(alkylene oxide) represented by the general formula (3) is, for example, a poly(alkylene oxide) having 1 to 10 carbon atoms. Specific examples of the poly(alkylene oxide) include poly(formaldehyde), poly(ethylene oxide), poly(n-propylene oxide), poly(n-butylene oxide), poly(n-pentyl oxide), poly(n-hexyl oxide), poly(n-heptyl oxide), poly(n-octyl oxide), poly(n-nonyl oxide) and poly(n-decyl oxide). Among these poly(alkylene oxides), poly(ethylene oxide) is preferred from the viewpoint of further improving Mg ion conductivity.

[0129] The multiple alkylene oxide structural units of the block represented by the general formula (3) are, for example, multiple alkylene oxide structural units having 1 to 10 carbon atoms. Specific examples of the alkylene oxide in the structural unit include methylene oxide, ethylene oxide, n-propoxy, n-butoxy, n-pentyloxy, n-hexyloxy, n-heptyloxy, n-octyloxy, n-nonyloxy and n-decyloxy. Among these alkylene oxides, ethylene oxide is preferred from the viewpoint of further improving Mg ion conductivity.

[0130] The anionic polymer preferably has a coordinating functional group in the main chain, as represented by the general formula (3). In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, the reason is presumed to be as follows. The coordinating functional group has a relatively flexible structure, so if the anionic polymer has a coordinating functional group in the main chain, the freedom of movement of the anionic polymer is improved. Electrostatic attraction acts on the anionic functional group and Mg 2+ Therefore, along with the movement of the main chain of the anionic polymer, Mg 2+ Therefore, if the anionic polymer has a coordinating functional group in the main chain, Mg 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0131] The coordinating functional group is preferably poly(alkylene oxide), more preferably poly(ethylene oxide) (poly(alkylene oxide) when q represents 2 in the general formula (3)). In this case, the Mg ion conductivity is further improved. Although not bound by a specific theory, it is speculated that the reason is as follows. Poly(ethylene oxide) has a relatively flexible structure, so if the anionic polymer has poly(ethylene oxide) as a coordinating functional group, the freedom of movement of the anionic polymer is improved. Furthermore, the lone pair of electrons of the oxygen atom of the polyalkylene oxide is easily coordinated to the Mg ion. 2+ Therefore, the Mg in the solid electrolyte 2+ The dispersibility of Mg is further improved. 2+ The ion transfer number is increased, and it is considered that the Mg ion conductivity is further improved.

[0132] The Mg polymer salt represented by the general formula (1) may be, for example, a Mg polymer salt represented by the general formula (5) (hereinafter, the Mg polymer salt represented by the general formula (5) is also referred to as "Mg polymer salt (5)").

[0133] [Chemistry 13]

[0134]

[0135] [In the general formula (5), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same as or different from each other.]

[0136] In addition, m, p, Af, n, and q in the general formula (5) are synonymous with m, p, Af in the general formula (2) and n and q in the general formula (3), respectively. In addition, as T in the general formula (5), for example, C6H5C(=S)S- can be cited. In addition, Af in the general formula (5) represents a monovalent anionic functional group.

[0137] The number average molecular weight Mn of the Mg polymer salt is, for example, 12,000 to 60,000. The method for measuring the number average molecular weight of the Mg polymer salt will be described in detail with reference to Examples.

[0138] Examples of the Mg polymer salt (5) include a Mg polymer salt represented by the general formula (5-2) (hereinafter also referred to as “Mg polymer salt (5-2)”).

[0139] [Chemistry 14]

[0140]

[0141] [In the general formula (5-2), m represents an integer of 3 to 40, and n represents an integer of 150 to 850.]

[0142] The solid electrolyte may also be composed of a Mg polymer salt.

[0143] In the electrochemical device of the present invention, the positive electrode is preferably a sulfur electrode composed of at least sulfur. In other words, the sulfur electrode of the electrochemical device of the present invention is preferably constituted as a positive electrode of sulfur (S) such as S8 and / or polymeric sulfur. The negative electrode is a magnesium electrode, and therefore, the electrochemical device of the present invention becomes an electrochemical device having a magnesium electrode-sulfur electrode pair, and has a solid electrolyte suitable therefor, thereby bringing about the desired cycle characteristics of such a positive electrode and being able to achieve an improvement in the coulombic efficiency of the negative electrode.

[0144] When the sulfur electrode is an electrode composed of at least sulfur, it may further contain a conductive additive and / or a binder, etc. In such a case, the sulfur content in the sulfur electrode may be 5 mass % or more and 95 mass % or less, preferably 70 mass % or more and 90 mass % or less, based on the entirety of the electrode.

[0145] For example, as the conductive aid contained in the sulfur electrode used as the positive electrode, carbon materials such as graphite, carbon fiber, carbon black, and carbon nanotubes can be cited, and one of them or a mixture of two or more thereof can be used. As carbon fiber, for example, vapor growth carbon fiber (Vapor Growth Carbon Fiber: VGCF (registered trademark)) can be used. As carbon black, for example, acetylene black and / or Ketjen black can be used. As carbon nanotubes, for example, single-walled carbon nanotubes (SWCNT) and / or multi-walled carbon nanotubes (MWCNT) such as double-walled carbon nanotubes (DWCNT) can be used. If it is a material with good conductivity, materials other than carbon materials can also be used, for example, metal materials such as Ni powder and / or conductive polymer materials can also be used. In addition, as a binder contained in the sulfur electrode used as a positive electrode, for example, a fluorine-based resin such as polyvinylidene fluoride (PVdF) and / or polytetrafluoroethylene (PTFE), a polyvinyl alcohol (PVA)-based resin, and / or a styrene-butadiene copolymer rubber (SBR)-based resin, etc. can be used. In addition, as a binder, a conductive polymer can also be used. As a conductive polymer, for example, substituted or unsubstituted polyaniline, polypyrrole, polythiophene, and a (co)polymer composed of one or two selected from them can be used.

[0146] On the other hand, in the electrochemical device of the present invention, the material constituting the negative electrode (specifically, the negative electrode active material) is a "magnesium electrode" and is therefore composed of a magnesium metal monomer, a magnesium alloy, or a magnesium compound. When the negative electrode is composed of a magnesium metal monomer (such as a magnesium plate, etc.), the Mg purity of the metal monomer is 90% or more, preferably 95% or more, and more preferably 98% or more. The negative electrode can be made of a plate-like material or a foil-like material, but is not limited thereto, and can also be formed (shaped) using powder.

[0147] The negative electrode may also have a structure in which a negative electrode active material layer is formed near its surface. For example, as the negative electrode active material layer, it may be a negative electrode having a layer having magnesium ion conductivity containing magnesium (Mg) and at least one of carbon (C), oxygen (O), sulfur (S) and halogen. This negative electrode active material layer is ultimately just an example, but it may also have a single peak from magnesium in the range of more than 40 eV and less than 60 eV. As the halogen, for example, at least one selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br) and iodine (I) may be cited. In this case, it may also be that from the surface of the negative electrode active material layer to 2×10 -7m, there is a single peak derived from magnesium in the range of 40 eV to 60 eV. This is because the negative electrode active material layer shows good electrochemical activity from its surface to the inside. In addition, for the same reason, it can also be that the oxidation state of magnesium is distributed from the surface of the negative electrode active material layer to the depth direction of 2×10 -7 nm is almost constant. Here, the surface of the negative electrode active material layer refers to the side of the surface of the electrode constituting the two sides of the negative electrode active material layer, and the back side refers to the side of the surface opposite to the surface, that is, the side of the interface constituting the collector and the negative electrode active material layer. Whether the negative electrode active material layer contains the above-mentioned elements can be confirmed based on the XPS (X-ray Photoelectron Spectroscopy) method. In addition, the negative electrode active material layer has the above-mentioned peak and the oxidation state of magnesium can also be confirmed in the same way based on the XPS method.

[0148] In the electrochemical device of the present invention, the positive electrode and the negative electrode are preferably separated by an inorganic or organic diaphragm that prevents the short circuit caused by the contact of the two poles and allows magnesium ions to pass. As inorganic diaphragms, for example, glass filters and glass fibers can be cited. As organic diaphragms, for example, porous films made of synthetic resins composed of polytetrafluoroethylene, polypropylene and / or polyethylene can be cited, and structures of two or more porous films stacked can also be formed. Among them, the porous film made of polyolefin has excellent anti-short circuit effect, and can achieve the safety improvement of the battery caused by the shutdown effect, so it is preferred.

[0149] The above-mentioned magnesium electrode-based electrochemical device can be configured as a secondary battery. The conceptual diagram in this case is as follows: Figure 1 As shown in the figure, during charging, magnesium ions (Mg 2+ ) moves from the positive electrode 10 to the negative electrode 11 through the electrolyte layer 12, converting electrical energy into chemical energy and storing electricity. During discharge, magnesium ions return from the negative electrode 11 to the positive electrode 10 through the electrolyte layer 12, generating electrical energy.

[0150] The electrochemical device can be made into a battery (primary battery or secondary battery) composed of the above-mentioned solid electrolyte of the present invention (hereinafter, also simply referred to as "electrolyte"), such a battery can be used as a driving power supply or auxiliary power supply for a notebook computer, PDA (portable information terminal), mobile phone, smart phone, cordless phone, camcorder, static digital camera, electronic book, electronic dictionary, portable music player, radio, earphone, game console, navigation system, memory card, pacemaker, hearing aid, power tool, electric shaver, refrigerator, air conditioner, television, stereo, water heater, microwave oven, dishwasher, washing machine, dryer, lighting equipment, toy, medical machine, robot, load regulator, traffic light, railway vehicle, golf cart, electric scooter and / or electric vehicle (including hybrid electric vehicle) etc. In addition, it can be carried as a power supply for power storage for buildings or power generation equipment represented by residences, or it can be used for supplying power to them. In electric vehicles, the conversion device that converts power into driving force by supplying power is usually a motor. As a control device (control unit) that performs information processing related to vehicle control, it includes a control device that displays the remaining battery capacity based on information related to the remaining battery capacity. In addition, batteries can also be used in power storage devices in so-called smart grids. Such power storage devices can not only supply electricity, but also store electricity by receiving power supply from other power sources. As other power sources, for example, thermal power generation, nuclear power generation, hydroelectric power generation, solar cells, wind power generation, geothermal power generation and / or fuel cells (including biofuel cells) can be used.

[0151] The electrochemical device (i.e., secondary battery) of the present invention can be applied to a secondary battery, a control unit (or control unit) that performs control related to the secondary battery, and a battery pack having an outer package containing the secondary battery. In such a battery pack, the control unit performs, for example, control of charging and discharging, overdischarging, or overcharging related to the secondary battery.

[0152] The electrochemical device (ie, secondary battery) of the present invention can also be applied to electronic devices that receive power supply from a secondary battery.

[0153] The electrochemical device (i.e., secondary battery) of the present invention can also be applied to an electric vehicle having a conversion device that receives power from a secondary battery and converts it into a driving force for the vehicle, and a control device (or control unit) that processes information related to vehicle control based on information related to the secondary battery. In such an electric vehicle, typically, the conversion device receives power from the secondary battery to drive the motor and generate driving force. Regenerative energy can also be used in the drive of the motor. In addition, the control device (or control unit) processes information related to vehicle control based on, for example, the remaining battery capacity of the secondary battery. Such electric vehicles include, for example, electric cars, electric motorcycles, electric bicycles, and railway vehicles, as well as so-called hybrid vehicles.

[0154] The electrochemical device of the present invention can also be applied to a secondary battery in a power system configured to receive power from a secondary battery and / or to supply power to a secondary battery from a power source. Such a power system can be any power system as long as it generally uses electricity, including a simple power device. Such a power system includes, for example, a smart grid, a home energy management system (HEMS) and / or a vehicle, and can also store electricity.

[0155] The electrochemical device (i.e., secondary battery) of the present invention can be applied to a power supply for storing electricity having a secondary battery and connected to an electronic device to which electricity is supplied. The use of such a power supply for storing electricity is not limited, and it can be used in basically any power system or power device, for example, it can be used in a smart grid.

[0156] Further details, further specific embodiments and other matters of the electrochemical device of the present invention are described in the above-mentioned [Solid electrolyte for electrochemical device of the present invention], and therefore, description thereof will be omitted to avoid duplication.

[0157] Here, the case where the magnesium electrode-based electrochemical device of the present invention is provided as a secondary battery will be described in further detail. Hereinafter, such a secondary battery is also referred to as a "magnesium secondary battery."

[0158] The magnesium secondary battery as the electrochemical device of the present invention is not particularly limited, and can be applied to machinery, equipment, appliances, devices, systems (a collection of multiple devices, etc.) that can use the magnesium secondary battery as a power source for driving, working, or a storage power source for power storage. The magnesium secondary battery used as a power source (for example, a magnesium-sulfur secondary battery) can also be a main power source (a power source used preferentially) or an auxiliary power source (a power source that replaces the main power source or is switched from the main power source). In the case where the magnesium secondary battery is used as an auxiliary power source, the main power source is not limited to the magnesium secondary battery.

[0159] Specific examples of the use of magnesium secondary batteries (particularly, magnesium-sulfur secondary batteries) include: video cameras, portable video cameras, digital still cameras, mobile phones, personal computers, televisions, various display devices, cordless phones, stereo headphones, music players, portable radios, electronic papers such as electronic books and / or electronic newspapers, various electronic devices such as portable information terminals including PDAs, electrical devices (including portable electronic devices); toys; portable living appliances such as electric shavers; lighting appliances such as room lamps; medical devices such as pacemakers and / or hearing aids Electronic devices; storage devices such as memory cards; battery packs used as detachable power sources for personal computers, etc.; power tools such as electric drills and / or electric saws; power storage systems such as home battery systems that store electricity for emergency use, home energy servers (home power storage devices), and power supply systems; power storage units and / or backup power supplies; electric vehicles such as electric cars, electric motorcycles, electric bicycles, and / or Segway (registered trademark); and the drive of electric drive force conversion devices (specifically, such as power motors) for aircraft and / or ships, but are not limited to these uses.

[0160] Among them, magnesium secondary batteries (especially magnesium-sulfur secondary batteries) are effectively applied to battery packs, electric vehicles, power storage systems, power supply systems, power tools, electronic equipment and / or electrical equipment. The battery pack is a power source using a magnesium secondary battery, which is a so-called assembled battery. An electric vehicle is a vehicle that uses a magnesium secondary battery as a driving power source to work (for example, drive), and can also be a car that has a driving source other than a secondary battery (for example, a hybrid car, etc.). A power storage system (for example, a power supply system) is a system that uses a magnesium secondary battery as a storage power source. For example, in a household power storage system (for example, a power supply system), since electricity is stored in a magnesium secondary battery as a storage power source, household electrical products can be used with electricity. Power tools are tools that use magnesium secondary batteries as a driving power source to make movable parts (such as drill bits, etc.) movable. Electronic equipment and electrical equipment are devices that use magnesium secondary batteries as a working power source (that is, a power supply source) to perform various functions.

[0161] Hereinafter, a cylindrical magnesium secondary battery and a flat-plate laminated film magnesium secondary battery will be described.

[0162] A schematic cross-sectional view of a cylindrical magnesium secondary battery 100 is shown in FIG. Figure 2As shown. In the magnesium secondary battery 100, an electrode structure 121 and a pair of insulating plates 112, 113 are housed inside a substantially hollow cylindrical electrode structure housing member 111. The electrode structure 121 can be made, for example, by winding the electrode structure after obtaining the electrode structure by stacking a positive electrode 122 and a negative electrode 124 via a separator 126. The electrode structure housing member (e.g., a battery can) 111 has a hollow structure with one end closed and the other end open, and is made of iron (Fe) and / or aluminum (Al), etc. A pair of insulating plates 112, 113 are configured to sandwich the electrode structure 121, and extend perpendicularly to the winding circumference of the electrode structure 121. The open end of the electrode structure storage member 111 is riveted with a battery cover 114, a safety valve mechanism 115 and a thermistor element (e.g., a PTC element, Positive Temperature Coefficient element) 116 via a gasket 117, thereby sealing the electrode structure storage member 111. The battery cover 114 is made of, for example, the same material as the electrode structure storage member 111. The safety valve mechanism 115 and the thermistor element 116 are arranged on the inner side of the battery cover 114, and the safety valve mechanism 115 is electrically connected to the battery cover 114 via the thermistor element 116. If the internal pressure becomes constant or above due to an internal short circuit and / or heating from the outside, the disc plate 115A in the safety valve mechanism 115 is flipped. As a result, the electrical connection between the battery cover 114 and the electrode structure 121 is cut off. In order to prevent abnormal heating caused by a large current, the resistance of the thermistor element 116 increases with the increase in temperature. The gasket 117 is made of, for example, an insulating material. The surface of the gasket 117 may be coated with asphalt or the like.

[0163] A center pin 118 is inserted into the winding center of the electrode structure 121. However, the center pin 118 does not have to be inserted to the winding center. A positive electrode lead portion 123 made of a conductive material such as aluminum is connected to the positive electrode 122. Specifically, the positive electrode lead portion 123 is mounted on the positive electrode collector. A negative electrode lead portion 125 made of a conductive material such as copper is connected to the negative electrode 124. Specifically, the negative electrode lead portion 125 is mounted on the negative electrode collector. The negative electrode lead portion 125 is welded to the electrode structure housing member 111 and is electrically connected to the electrode structure housing member 111. The positive electrode lead portion 123 is welded to the safety valve mechanism 115 and is electrically connected to the battery cover 114. In addition, at Figure 2 In the example shown, the negative electrode lead portion 125 is provided at one location (the outermost peripheral portion of the wound electrode structure), but may be provided at two locations (the outermost peripheral portion and the innermost peripheral portion of the wound electrode structure).

[0164] The electrode structure 121 is composed of a positive electrode 122 having a positive electrode active material layer formed on a positive electrode collector (more specifically, on both sides of the positive electrode collector) and a negative electrode 124 having a negative electrode active material layer formed on a negative electrode collector (more specifically, on both sides of the negative electrode collector) stacked via a separator 126. The positive electrode active material layer is not formed in the region of the positive electrode collector to which the positive electrode lead portion 123 is attached, and the negative electrode active material layer is not formed in the region of the negative electrode collector to which the negative electrode lead portion 125 is attached.

[0165] The magnesium secondary battery 100 can be manufactured, for example, according to the following steps.

[0166] First, a positive electrode active material layer is formed on both surfaces of a positive electrode current collector, and a negative electrode active material layer is formed on both surfaces of a negative electrode current collector.

[0167] Next, the positive electrode lead portion 123 is installed on the positive electrode collector using a welding method or the like. In addition, the negative electrode lead portion 125 is installed on the negative electrode collector using a welding method or the like. Next, the positive electrode 122 and the negative electrode 124 are stacked and wound via a separator 126 composed of a microporous polyethylene film (more specifically, an electrode structure (i.e., a stacked structure) of the positive electrode 122 / separator 126 / negative electrode 124 / separator 126 is wound), and after the electrode structure 121 is produced, a protective tape (not shown) is affixed to the outermost portion. Thereafter, a center pin 118 is inserted into the center of the electrode structure 121. Next, the electrode structure 121 is clamped by a pair of insulating plates 112 and 113, and the electrode structure 121 is housed inside the electrode structure housing member 111. In this case, the front end of the positive electrode lead portion 123 is attached to the safety valve mechanism 115 by welding or the like, and the front end of the negative electrode lead portion 125 is attached to the electrode structure housing member 111. Thereafter, the electrolyte is injected based on the reduced pressure method so that the electrolyte is impregnated into the separator 126. Next, the battery cover 114, the safety valve mechanism 115, and the thermistor element 116 are riveted to the open end of the electrode structure housing member 111 via the gasket 117.

[0168] Next, a flat-plate laminated film type secondary battery is described. A schematic exploded perspective view of such a secondary battery is shown in FIG. Figure 3As shown. In this secondary battery, an electrode structure 221 substantially the same as above is housed inside an outer packaging member 200 composed of a laminated film. The electrode structure 221 can be made by winding the stacked structure after stacking the positive electrode and the negative electrode via a separator and an electrolyte layer. A positive electrode lead portion 223 is installed on the positive electrode, and a negative electrode lead portion 225 is installed on the negative electrode. The outermost periphery of the electrode structure 221 is protected by a protective tape. The positive electrode lead portion 223 and the negative electrode lead portion 225 protrude in the same direction from the inside of the outer packaging member 200 toward the outside. The positive electrode lead portion 223 is formed of a conductive material such as aluminum. The negative electrode lead portion 225 is formed of a conductive material such as copper, nickel and / or stainless steel.

[0169] The outer packaging member 200 is capable of Figure 3 A film folded in the direction of the arrow R shown, a depression (e.g., embossing) for accommodating the electrode structure 221 is provided in a part of the outer packaging member 200. The outer packaging member 200 is, for example, a laminated film obtained by sequentially stacking a welding layer, a metal layer, and a surface protection layer. In the manufacturing process of the secondary battery, after the outer packaging member 200 is folded in a manner that the welding layers are opposite to each other across the electrode structure 221, the outer peripheral edges of the welding layers are welded to each other. However, the outer packaging member 200 can also be bonded to two separate laminated films by an adhesive or the like. The welding layer is, for example, composed of a film of polyethylene and / or polypropylene. The metal layer is, for example, composed of aluminum foil. The surface protection layer is, for example, composed of nylon and / or polyethylene terephthalate. Among them, the outer packaging member 200 is preferably an aluminum laminated film in which a polyethylene film, an aluminum foil, and a nylon film are sequentially stacked. However, the outer packaging member 200 can also be a laminated film having other laminated structures, a polymer film such as polypropylene, or a metal film. Specifically, the film may be composed of a moisture-resistant aluminum laminate film obtained by laminating a nylon film, an aluminum foil, and an unstretched polypropylene film in this order from the outside.

[0170] In order to prevent the intrusion of external air, a close-fitting film 201 is inserted between the outer packaging member 200 and the positive lead portion 223 and between the outer packaging member 200 and the negative lead portion 225. The close-fitting film 201 may also be made of a material having close adhesion to the positive lead portion 223 and the negative lead portion 225, such as a polyolefin resin, and more specifically, may be made of a polyolefin resin such as polyethylene, polypropylene, modified polyethylene, and modified polypropylene.

[0171] In the above, the description is mainly about secondary batteries, but the present disclosure is also applicable to other electrochemical devices such as capacitors, air batteries, and fuel cells, etc. This will be described below.

[0172] Figure 4The electrochemical device of the present invention can be provided as a capacitor as shown in a schematic cross-sectional view. In the capacitor, a positive electrode 31 and a negative electrode 32 are arranged opposite to each other via a separator 33 containing an electrolyte. Reference numerals 35 and 36 denote current collectors, and reference numeral 37 denotes a gasket.

[0173] Or, if Figure 5 As shown in the conceptual diagram of , the electrochemical device of the present invention can also be provided as an air battery. The above-mentioned air battery is composed of the following components: an oxygen selective permeable membrane 47 that makes it difficult for water vapor to pass through and selectively allows oxygen to pass through; an air electrode side collector 44 composed of a conductive porous material; a porous diffusion layer 46 arranged between the air electrode side collector 44 and the porous positive electrode 41 and composed of a conductive material; a porous positive electrode 41 containing a conductive material and a catalyst material; a diaphragm that is difficult for water vapor to pass through and a solid electrolyte (or a solid electrolyte containing a solid electrolyte) 43; a negative electrode 42 that releases magnesium ions; a negative electrode side collector 45; and an outer packaging body 48 that accommodates these layers.

[0174] Oxygen 52 in air (e.g., atmosphere) 51 selectively permeates through the oxygen selective permeable membrane 47, passes through the air electrode side current collector 44 made of a porous material, diffuses through the diffusion layer 46, and is supplied to the porous positive electrode 41. The advance of oxygen that permeates the oxygen selective permeable membrane 47 is partially blocked by the air electrode side current collector 44, but the oxygen that has passed through the air electrode side current collector 44 is diffused by the diffusion layer 46, and due to the diffusion, it efficiently spreads throughout the entire porous positive electrode 41, and the supply of oxygen to the entire surface of the porous positive electrode 41 is not hindered by the air electrode side current collector 44. In addition, since the permeation of water vapor is suppressed by the oxygen selective permeable membrane 47, the deterioration caused by the influence of moisture in the air is less, and oxygen is efficiently supplied to the entire porous positive electrode 41, so that the battery output can be improved and stable long-term use can be achieved.

[0175] In addition, regarding the negative electrode in the electrochemical device, in addition to being able to use the Mg metal plate, it can also be manufactured by the following method. For example, a Mg solid electrolyte (Mg-EnPS) containing MgCl2 and EnPS (ethyl n-propyl sulfone) is prepared, and the Mg solid electrolyte is used to precipitate Mg metal on Cu foil based on the electroplating method, and a Mg coating can be formed on Cu foil as a negative electrode active material layer. In addition, the surface of the Mg coating obtained by the above method is analyzed based on the XPS method. As a result, Mg, C, O, S and Cl are present on the surface of the Mg coating. In addition, the peak from Mg observed in the surface analysis is not split, and a single peak from Mg is observed in the range of more than 40eV and less than 60eV. Furthermore, based on the Ar sputtering method, about 200nm is dug into the depth direction of the surface of the Mg coating, and its surface is analyzed based on the XPS method. As a result, the position and shape of the peak from Mg after Ar sputtering are compared with the position and shape of the peak before Ar sputtering. There is no change.

[0176] As reference Figure 1 to Figure 3 As described above, the electrochemical device of the present invention can be used particularly as a magnesium secondary battery, and several application examples of the magnesium secondary battery will be described in more detail. In addition, the configuration of each application example described below is ultimately an example, and the configuration can be appropriately changed.

[0177] The magnesium secondary battery can be used in the form of a battery pack. The battery pack is a simple battery pack (so-called soft package) using a magnesium secondary battery, for example, mounted on electronic devices represented by smartphones. Alternatively or on the basis of this, a battery pack may be provided with 6 magnesium secondary batteries connected in 2 parallel and 3 series. In addition, the connection form of the magnesium secondary battery may be in series, in parallel, or a mixture of the two.

[0178] Figure 6 A block diagram showing an example of a circuit configuration in which the magnesium secondary battery of the present invention is applied to a battery pack is shown. The battery pack includes a battery cell (e.g., an assembled battery) 1001, an outer packaging member, a switch unit 1021, a current detection resistor 1014, a temperature detection element 1016, and a control unit 1010. The switch unit 1021 includes a charging control switch 1022 and a discharge control switch 1024. In addition, the battery pack includes a positive terminal 1031 and a negative terminal 1032. When charging, the positive terminal 1031 and the negative terminal 1032 are respectively connected to the positive terminal and the negative terminal of the charger for charging. In addition, when the electronic device is used, the positive terminal 1031 and the negative terminal 1032 are respectively connected to the positive terminal and the negative terminal of the electronic device for discharge.

[0179] The battery unit 1001 is formed by connecting a plurality of magnesium secondary batteries 1002 of the present disclosure in series and / or in parallel. Figure 6 , six magnesium secondary batteries 1002 are connected in a 2-in-parallel and 3-in-series (2P3S) manner, but any other connection method may be used, such as p-in-parallel and q-in-series (where p and q are integers).

[0180] The switch unit 1021 includes a charge control switch 1022 and a diode 1023 and a discharge control switch 1024 and a diode 1025, and is controlled by the control unit 1010. The diode 1023 has a polarity opposite to the charge current flowing from the positive terminal 1031 to the battery cell 1001 and in the same direction as the discharge current flowing from the negative terminal 1032 to the battery cell 1001. The diode 1025 has a polarity in the same direction as the charge current and in the opposite direction to the discharge current. In addition, in the example, the switch unit is set on the positive (+) side, but it can also be set on the negative (-) side. The charge control switch 1022 is controlled by the control unit 1010 so that it becomes an off state when the battery voltage becomes an overcharge detection voltage, and no charging current flows in the current path of the battery cell 1001. After the charge control switch 1022 becomes an off state, it is possible to discharge only through the diode 1023. Furthermore, the control unit 1010 controls the control switch 1024 so that it is turned off when a large current flows during charging, and the charging current flowing through the current path of the battery cell 1001 is cut off. The control unit 1010 controls the discharge control switch 1024 so that it is turned off when the battery voltage reaches the over-discharge detection voltage, and the discharge current does not flow through the current path of the battery cell 1001. After the discharge control switch 1024 is turned off, only charging is possible through the diode 1025. Furthermore, the control unit 1010 controls the control switch 1024 so that it is turned off when a large current flows during discharging, and the discharge current flowing through the current path of the battery cell 1001 is cut off.

[0181] The temperature detection element 1016 is composed of, for example, a thermistor and is provided near the battery cell 1001. The temperature measuring unit 1015 measures the temperature of the battery cell 1001 using the temperature detection element 1016 and transmits the measurement result to the control unit 1010. The voltage measuring unit 1012 measures the voltage of the battery cell 1001 and the voltage of each magnesium secondary battery 1002 constituting the battery cell 1001, performs A / D conversion on the measurement result and transmits it to the control unit 1010. The current measuring unit 1013 measures the current using the current detection resistor 1014 and transmits the measurement result to the control unit 1010.

[0182] The switch control unit 1020 controls the charge control switch 1022 and the discharge control switch 1024 of the switch unit 1021 based on the voltage and current sent from the voltage measuring unit 1012 and the current measuring unit 1013. When the voltage of any of the magnesium secondary batteries 1002 becomes less than the overcharge detection voltage or the overdischarge detection voltage and / or when a large current flows rapidly, the switch control unit 1020 prevents overcharge and overdischarge, and overcurrent charge and discharge by sending a control signal to the switch unit 1021. The charge control switch 1022 and the discharge control switch 1024 can be formed by a semiconductor switch such as MOSFET, for example. In this case, the diodes 1023 and 1025 are formed by the parasitic diode of the MOSFET. When a p-channel FET is used as the MOSFET, the switch control unit 1020 supplies a control signal DO and a control signal CO to the gate of each of the charge control switch 1022 and the discharge control switch 1024. The charge control switch 1022 and the discharge control switch 1024 are turned on by a gate potential that is lower than the source potential by a predetermined value or more. That is, in normal charging and discharging operations, the control signals CO and DO are set to low levels to turn on the charging control switch 1022 and the discharging control switch 1024. In addition, for example, in overcharging or overdischarging, the control signals CO and DO are set to high levels to turn off the charging control switch 1022 and the discharging control switch 1024.

[0183] The memory 1011 is composed of, for example, an EPROM (Erasable Programmable Read Only Memory) as a non-volatile memory. The memory 1011 stores in advance the values ​​calculated by the control unit 1010 and / or the internal resistance value of each magnesium secondary battery 1002 in the initial state measured in the manufacturing process, and can be rewritten as appropriate. In addition, by pre-storing the full charge capacity of the magnesium secondary battery 1002, for example, the remaining capacity can be calculated together with the control unit 1010.

[0184] The temperature measuring unit 1015 measures the temperature using the temperature detection element 1016 , performs charge and discharge control when abnormal heat generation occurs, and performs correction in the calculation of the remaining capacity.

[0185] Next, application of the magnesium secondary battery to electric vehicles will be described. Figure 7A is a block diagram showing the structure of an electric vehicle such as a hybrid vehicle as an example of an electric vehicle. The electric vehicle includes, for example, a control unit 2001, various sensors 2002, a power supply 2003, an engine 2010, a generator 2011, inverters 2012 and 2013, a driving motor 2014, a differential device 2015, a transmission 2016, and a clutch 2017 inside a metal housing 2000. In addition, the electric vehicle includes, for example, a front wheel drive shaft 2021 connected to the differential device 2015 and / or the transmission 2016, a front wheel 2022, a rear wheel drive shaft 2023, and a rear wheel 2024.

[0186] The electric vehicle can travel with either the engine 2010 or the motor 2014 as a driving source. The engine 2010 is a main power source, such as a gasoline engine. When the engine 2010 is used as a power source, the driving force (such as the rotational force) of the engine 2010 is transmitted to the front wheel 2022 or the rear wheel 2024 via the differential device 2015, the transmission 2016 and the clutch 2017 as a driving unit. The rotational force of the engine 2010 is also transmitted to the generator 2011, and the generator 2011 generates AC power using the rotational force. The AC power is converted into DC power via the inverter 2013 and stored in the power supply 2003. On the other hand, when the motor 2014 as a conversion unit is used as a power source, the power (such as DC power) supplied from the power supply 2003 is converted into AC power via the inverter 2012, and the motor 2014 is driven by the AC power. The driving force (eg, rotational force) converted from the electric power by the motor 2014 is transmitted to the front wheels 2022 or the rear wheels 2024 via, for example, the differential device 2015 , the transmission 2016 , and the clutch 2017 as a driving unit.

[0187] Alternatively, when the electric vehicle is decelerated by a brake mechanism (not shown), the resistance force during deceleration is transmitted as a rotational force to the motor 2014, and the motor 2014 generates AC power using the rotational force. The AC power is converted into DC power by the inverter 2012, and the DC regenerative power is stored in the power supply 2003.

[0188] The control unit 2001 controls the overall operation of the electric vehicle, and includes, for example, a CPU. The power supply 2003 may include one or more magnesium secondary batteries (not shown) of the present invention. The power supply 2003 may also be connected to an external power supply and store power by receiving power supply from the external power supply. The various sensors 2002 are used, for example, to control the speed of the engine 2010 and control the opening (throttle opening) of the throttle valve (not shown). The various sensors 2002 include, for example, a speed sensor, an acceleration sensor, and / or an engine speed sensor.

[0189] Furthermore, although the electric vehicle is described as a hybrid vehicle, the electric vehicle may be a vehicle that operates without using the engine 2010 but only using the power source 2003 and the motor 2014 (for example, an electric car).

[0190] Next, application of the magnesium secondary battery to a power storage system (for example, a power supply system) will be described. Figure 7 B is a block diagram showing the configuration of a power storage system (eg, power supply system). The power storage system includes a control unit 3001, a power supply 3002, a smart meter 3003, and a power hub 3004 inside a house 3000 such as a general residence or a commercial building.

[0191] The power source 3002 is connected to an electrical device (e.g., electronic device) 3010 disposed inside the house 3000, and can be connected to an electric vehicle 3011 parked outside the house 3000. In addition, the power source 3002 is connected to a self-generating generator 3021 disposed in the house 3000, for example, via a power hub 3004, and can be connected to an external centralized power system 3022 via a smart meter 3003 and a power hub 3004. The electrical device (e.g., electronic device) 3010 includes, for example, one or more household appliances. As household appliances, for example, a refrigerator, an air conditioner, a television, and / or a water heater can be cited. The self-generating generator 3021 is composed of, for example, a solar power generator and / or a wind power generator. As the electric vehicle 3011, for example, an electric car, a hybrid car, an electric motorcycle, an electric bicycle, and / or a Segway (registered trademark) can be cited. Examples of the centralized power system 3022 include commercial power supplies, power generation devices, power transmission networks and / or smart grids (for example, next-generation power transmission networks). In addition, examples include thermal power plants, nuclear power plants, hydroelectric power plants and / or wind power plants. Examples of power generation devices included in the centralized power system 3022 include various solar cells, fuel cells, wind power generation devices and / or micro-hydroelectric power generation devices, geothermal power generation devices, etc., but are not limited to these.

[0192] The control unit 3001 controls the overall operation of the power storage system (including the use status of the power supply 3002), and includes, for example, a CPU. The power supply 3002 may include one or more magnesium secondary batteries (not shown) according to the present invention. The smart meter 3003 is, for example, a network-compatible power meter provided in the house 3000 on the power demand side, and is capable of communicating with the power supply side. Moreover, the smart meter 3003 can achieve efficient and stable energy supply by, for example, controlling the balance between demand and supply in the house 3000 while communicating with the outside.

[0193] In the above power storage system, for example, power is stored in the power source 3002 from the centralized power system 3022 as an external power source via the smart meter 3003 and the power concentrator 3004, and power is stored in the power source 3002 from the self-generating generator 3021 as an independent power source via the power concentrator 3004. The power stored in the power source 3002 is supplied to the electrical device (e.g., electronic device) 3010 and the electric vehicle 3011 according to the instruction of the control unit 3001, so that the electrical device (e.g., electronic device) 3010 can be operated and the electric vehicle 3011 can be charged. That is, the power storage system is a system that can store and supply power in the house 3000 using the power source 3002.

[0194] The power stored in the power source 3002 can be used arbitrarily. Therefore, for example, power can be stored in the power source 3002 from the centralized power system 3022 at night when the power rate is low, and the power stored in the power source 3002 can be used during the day when the power rate is high.

[0195] The power storage system described above may be installed for each household (for example, one family) or for each plurality of households (for example, a plurality of families).

[0196] Next, application of the magnesium secondary battery to an electric power tool will be described. Figure 7 C shows a block diagram showing the structure of an electric tool. The electric tool is, for example, an electric drill, and includes a control unit 4001 and a power source 4002 inside a tool body 4000 made of a plastic material or the like. A drill head 4003 as a movable part is rotatably mounted on the tool body 4000, for example. The control unit 4001 controls the overall operation of the electric tool (including the use status of the power source 4002), and includes, for example, a CPU or the like. The power source 4002 can include one or more magnesium secondary batteries (not shown) involved in the present invention. The control unit 4001 supplies power from the power source 4002 to the drill head 4003 according to the operation of an action switch (not shown).

[0197] Although the embodiments of the present invention have been described above, these are merely typical examples, and therefore, the present invention is not limited thereto, and it is easily understood by those skilled in the art that various embodiments can be considered without changing the gist of the present invention.

[0198] For example, the composition of the solid electrolyte, raw materials used for production, production methods, production conditions, properties of the solid electrolyte, electrochemical devices, and the configuration or structure of the battery described above are merely illustrative and are not limited thereto, and may be appropriately modified.

[0199] Example

[0200] Hereinafter, the present invention will be described in more detail using Examples, but the present invention is not limited to these Examples.

[0201] [Example]

[0202] [1. Synthesis of Mg polymer salt]

[0203] Mg polymer salt (5-2) was synthesized.

[0204] In the synthesis of the Mg polymer salt (5-2), the following reagents were used.

[0205] ·Magnesium chloride (MgCl2) (anhydrous): manufactured by Sigma-Aldrich

[0206] · Magnesium bis(trifluoromethanesulfonyl)imide (Mg(TFSI)2): Made by Toyama Pharmaceutical Industries

[0207] ·Dimethoxyethane (DME): Made by Toyama Pharmaceutical Industries

[0208] Potassium 3-(methacryloyloxy)propane-1-sulfonate: manufactured by Sigma-Aldrich, 98%

[0209] Anhydrous tetrahydrofuran (anhydrous THF): Made by Sigma-Aldrich, anhydrous, no inhibitors, ≥99.9%

[0210] ·Thionyl chloride (SOCl2): Nacalai Tesque, special grade, >99%

[0211] Anhydrous dimethylformamide (anhydrous DMF): manufactured by Sigma-Aldrich, anhydrous, 99.8%

[0212] Dichloromethane (DCM): Made by Nacalai Tesque, JIS reagent special grade, ≥99.5% (GC)

[0213] Anhydrous magnesium sulfate (anhydrous MgSO4): Made by Nacalai Tesque, Nacalai standard grade 1, ≥99.0% (after strong heating)

[0214] ·Trifluoromethanesulfonamide (CF3SO2NH2): manufactured by Tokyo Chemical Industry, >98.0% (T)

[0215] Anhydrous triethylamine: Sigma-Aldrich, ≥99.5%, ≤0.1% (Karl Fischer)

[0216] ·4-Methoxyphenol: Made by Tokyo Chemical Industry, 99%

[0217] Lithium hydride (LiH): Sigma-Aldrich, powder, -30 mesh, 95%

[0218] Hexane: Sigma-Aldrich, ReagentPlus(R), ≥99%

[0219] Poly(ethylene oxide) (PEO): manufactured by Sigma-Aldrich, Mw = 35000 g / mol

[0220] Anhydrous dichloromethane (DCM): Made by Sigma-Aldrich, containing 40-150 ppm pentene as a stabilizer, ≥99.8%

[0221] ·4-Cyano-4-(thiobenzylthio)pentanoic acid (CPADB): manufactured by Sigma-Aldrich, >97.0%

[0222] N,N-Dicyclohexylcarbodiimide (DCC): manufactured by Sigma-Aldrich, >99.0%

[0223] ·4-(Dimethylamino)pyridine (DMAP): Sigma-Aldrich, ≥99.0%

[0224] Ether: Nacalai Tesque, JIS reagent special grade, ≥99.5%

[0225] ·2,2'-Azobis(2-aminopropane) hydrochloride (AIBA): manufactured by Tokyo Chemical Industry, >98.0% (HPLC)

[0226] Dialysis membrane: Thermo Fisher Scientific, 3500-MW cut-off (MWCO), regenerated cellulose dialysis membrane

[0227] The Mg polymer salt (5-2) is synthesized according to reactions (r-1) to (r-2) as shown in the following reaction scheme.

[0228] [Chemistry 15]

[0229]

[0230] In reaction (r-1), in the presence of polymerization initiator AIBA, PEO macrochain transfer agent (6-2) and Li salt of sulfonyl imide derivative (7-2) are subjected to reversible addition-fragmentation chain polymerization reaction to synthesize Li polymer salt (4-2). Next, in reaction (r-2), Mg polymer salt (5-2) is synthesized by ion exchange reaction of Li polymer salt (4-2). In addition, m and n in chemical formulas (4-2) and (5-2) respectively represent the degree of polymerization of the repeating units represented by chemical formulas (4-2) and (5-2). m is about 33 to 34, and n is about 794 to 795. In addition, n in chemical formula (6-2) is synonymous with n in chemical formula (5-2). The synthesis of Mg polymer salt (5-2) is described in detail below.

[0231] [1-1. Synthesis of Li Salt of Sulfonyl Imide Derivative (7-2)]

[0232] The Li salt of the sulfonyl imide derivative (7-2) was synthesized according to reactions (r-3) to (r-5).

[0233] [Chemistry 16]

[0234]

[0235] (Reaction (r-3): Synthesis of 3-(chlorosulfonyl)propyl methacrylate (sulfonyl chloride (b))

[0236] According to reaction (r-3), the sulfonate (a) is chlorinated to obtain the sulfonyl chloride (b).

[0237] Specifically, 15.00 g (0.06 mol) of potassium 3-(methacryloyloxy) propane-1-sulfonate was dried under reduced pressure and added to 25 mL of anhydrous THF under an argon atmosphere to form a suspension. 39.90 g (0.34 mol) of thionyl chloride as a chlorinating agent was dissolved in 1.7 mL of anhydrous DMF to prepare a DMF solution of thionyl chloride. While the suspension was ice-cooled and stirred with a stirrer, a DMF solution of thionyl chloride was added dropwise under an argon atmosphere. Stirring was performed under the conditions of 0°C for 1 hour and then at room temperature (e.g., 25°C) for 15 hours. Thereafter, cold water was added little by little to 200 mL. 80 mL of dichloromethane was added, and after washing 6 times in 25 mL of distilled water, the dichloromethane phase was dried using anhydrous MgSO4. The dichloromethane phase was filtered, and the desiccant was filtered out and removed. The filtrate was dried under reduced pressure using an evaporator, and dichloromethane was distilled off to obtain a residue. Thereafter, the residue was dried under reduced pressure overnight to obtain sulfonyl chloride (b).

[0238] (Reaction (r-4): Triethylammonium-1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide) (Synthesis of tertiary ammonium salt of sulfonimide derivative (c))

[0239] According to the reaction (r-4), a tertiary ammonium salt (c) of a sulfonylimide derivative is obtained by an addition elimination reaction of the sulfonyl chloride (b) with trifluoromethanesulfonamide as a nucleophile.

[0240] Specifically, 10.90 g (0.11 mol) of anhydrous triethylamine was slowly added to 7.30 g (0.05 mol) of trifluoromethanesulfonamide under an argon atmosphere while stirring with a stirrer, and then 40 mL of anhydrous THF was added to obtain a solution.

[0241] 11.10 g (0.05 mol) of sulfonyl chloride (b) was mixed with 15 mL (13.50 g) of anhydrous THF to prepare a THF solution of sulfonyl chloride (b). The THF solution of sulfonyl chloride (b) was slowly added dropwise to the solution while the solution was ice-cooled and stirred with a stirrer. Thereafter, the mixture was stirred with a stirrer at 0°C for 1 hour, returned to room temperature, and stirred with a stirrer at room temperature for 1 hour. Thus, a precipitate was obtained.

[0242] The precipitate was filtered by suction under an argon atmosphere. Thereafter, the filtrate was dried under reduced pressure using an evaporator. 90 mL of dichloromethane was added, and after washing 4 times in 35 mL of distilled water, the dichloromethane phase was dried using anhydrous MgSO4. The dichloromethane phase was filtered, and the desiccant was filtered out and removed. After adding a small amount of 4-methoxyphenol to the filtrate, the dichloromethane of the filtrate was distilled out using an evaporator to obtain a residue. Thereafter, the residue was dried under reduced pressure to obtain a tertiary ammonium salt (c) of a sulfonylimide derivative.

[0243] (Reaction (r-5): Synthesis of lithium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide) (Li salt of sulfonyl imide derivative (7-2))

[0244] In the reaction (r-5), the Li salt (7-2) of the sulfonyl imide derivative is obtained by an ion exchange reaction of the tertiary ammonium salt (c) of the sulfonyl imide derivative.

[0245] Specifically, while stirring 9 mL of anhydrous THF with a stirrer under an argon atmosphere, 5.89 g (13.36 mmol) of a tertiary ammonium salt (c) of a sulfonyl imide derivative was added. Thereafter, 0.26 g (34.06 mmol) of LiH was further added little by little. Stirring was performed with a stirrer under an argon atmosphere overnight. Thereafter, the mixture was filtered, and the filtrate was concentrated under reduced pressure by an evaporator to obtain a residue. The residue was washed 4 times with 10 mL of n-hexane. Thereafter, the residue was further dried under reduced pressure. 25 mL of anhydrous dichloromethane was added to the residue and refrigerated (10° C.) overnight to allow the precipitate to precipitate. The precipitate was filtered and dried under reduced pressure to obtain the Li salt (7-2) of the sulfonyl imide derivative.

[0246] [1-2. Synthesis of PEO macrochain transfer agent]

[0247] According to reaction (r-6), CPADB and PEO are subjected to a Steglich esterification reaction to obtain a PEO macrochain transfer agent (6-2).

[0248] [Chemistry 17]

[0249]

[0250] Specifically, 15.0 g of PEO was distilled for 2 hours using 30 mL of toluene. Thereafter, it was dried under reduced pressure at 55 ° C for 12 hours. 10.00 g (0.29 mmoL) of PEO was dissolved in 100 mL of anhydrous dichloromethane (DCM) to prepare a DCM solution of PEO. 0.95 g (3.42 mmoL) of 4-cyano-4-(thiobenzoylthio) valeric acid (CPADB) was dispersed in 0.77 g (3.76 mmoL) of N, N-dicyclohexylcarbodiimide (DCC) as a condensing agent to prepare a dispersion. While stirring the DCM solution of PEO with a stirrer at 0 ° C, the dispersion was slowly added dropwise to the DCM solution of PEO.

[0251] 0.13 g (1.06 mmol) of 4-(dimethylamino)pyridine (DMAP) as a catalyst was dissolved in 2 mL of anhydrous DCM to prepare a DCM solution of DMAP. The DCM solution of DMAP was further added dropwise to the DCM solution of PEO, and stirred with a stirrer at 0°C for 48 hours. Thereafter, the solid was filtered out and washed with 50 mL of DCM. 500 mL of ice-cold ether was added to the filtrate to precipitate the polymer, which was then centrifuged. 30 mL of DCM was added to the separated polymer and dissolved, and the operation of centrifuging with 100 mL of ice-cold ether was repeated twice. PEO macro-chain transfer agent (macro-CTA) (6-2) was obtained by drying under reduced pressure at room temperature for 3 hours.

[0252] [1-3. Synthesis of Li polymer salt (4-2)]

[0253] According to reaction (r-1), a PEO macrochain transfer agent (6-2) and a Li salt (d) of a sulfonimide derivative undergo a reversible addition-fragmentation chain polymerization reaction to obtain a Li polymer salt (4-2).

[0254] Specifically, 0.70 g (20 μmole) of a PEO macrochain transfer agent (6-2) and 0.47 g (1.35 mmoL) of a Li salt (d) of a sulfonyl imide derivative were dissolved in 4.7 mL of ion exchange water to prepare a solution. 1.09 mg (4.02 μmole) of AIBA as a polymerization initiator was added to the obtained solution and dissolved. After argon replacement, it was immersed in an oil bath heated to 65°C and heated for 11 hours. It was returned to room temperature and dialyzed with distilled water for 3 days (MWCO 3500). Dialysis and freeze drying were performed, and reduced pressure drying was performed at 80°C for 24 hours to obtain a Li polymer salt (4-2).

[0255] [1-4. Synthesis of Mg polymer salt (5-2)]

[0256] According to the reaction (r-2), the Mg polymer salt (5-2) is synthesized. In the reaction (r-2), the Mg polymer salt (5-2) is obtained by an ion exchange reaction of the Li polymer salt (4-2).

[0257] Specifically, the Li polymer salt (4-2) (thickness t = 100 μm, 0.05 g) which was made into a sheet and dried under reduced pressure under an argon atmosphere was dissolved in 2 mL of a Mg electrolyte ((2M MgCl2 + 1M Mg(TFSI)2) / DME). 38 mL of DME was further added to precipitate the Mg polymer salt (5-2). The supernatant was removed, and the solid was washed twice with 20 mL of DME. Thereafter, it was naturally dried under an argon atmosphere. Thereafter, it was dried under reduced pressure (room temperature, 1 hour) and hot pressed to form a sheet.

[0258] [1-5. Identification]

[0259] The obtained Li polymer salt (4-2) and Mg polymer salt (5-2) were measured. 1 NMR spectrum. In addition, 1 In the measurement of NMR spectrum, CDCl3 was used as a solvent and tetramethylsilane (TMS) was used as an internal standard sample.

[0260] Fig. 9 (a) shows the Mg polymer salt (5-2) 1 NMR spectroscopy, Fig. 9 (b) shows the Li polymer salt (4-2) 1 NMR spectra. The chemical structural formulas of these polymer salts are also shown. Fig. 9 In (b), 1 Each peak of the NMR spectrum is attributed to the hydrogen atom of the Li polymer salt (4-2). 1 The peak values ​​of the NMR spectrum and the numerical values ​​in the chemical structure formula represent the corresponding relationship. Thus, it was confirmed that the target Li polymer salt (4-2) could be synthesized. In addition, Fig. 9 In (a), the same 1 Each peak of the NMR spectrum is attributed to the hydrogen atoms of the Mg polymer salt (5-2). Fig. 9 (a) 1 NMR spectra relative to Fig. 9 (b) 1 NMR spectra have almost the same shape, so it is confirmed that even if Li + Replaced by Mg 2+ There will be no structural change in the counter anion (anionic polymer).

[0261] (Determination of number average molecular weight Mn)

[0262] The number average molecular weight Mn of the Mg polymer salt (5-2) was determined by gel permeation chromatography. The measurement conditions were 0.1 M MgCl2-1.5×10 -5 M NaN 3 A solution of 400 μL was used as an eluent, and a mixed solvent of water / acetonitrile (4 / 1=v / v) was used as a solvent of the solution. The flow rate of the eluent was 0.5 mL / min at 35° C. A pullulan standard was used for calibration.

[0263] [2. Fabrication of polymer solid electrolyte and magnesium-sulfur secondary battery]

[0264] A polymer solid electrolyte and a magnesium-sulfur secondary battery comprising the electrolyte were produced. The specifications of the polymer solid electrolyte and the magnesium-sulfur secondary battery are as follows.

[0265] (Specifications of polymer solid electrolyte)

[0266] Mg polymer salt (5-2) (Ø5mm, thickness t100μm)

[0267] (Specifications of magnesium-sulfur secondary batteries)

[0268] ●Negative electrode: magnesium electrode (Mg plate with diameter 15 mm and thickness 200 μm / purity 99.9%)

[0269] Positive electrode: Sulfur electrode (electrode containing 10 mass % S8 sulfur, Ketjen black (KB) as a conductive additive, and polytetrafluoroethylene (PTFE) as a binder)

[0270] ●Diaphragm: Glass fiber

[0271] ●Polymer solid electrolyte: Mg polymer salt (5-2) (Ф5mm)

[0272] ● Secondary battery form: Button battery CR2016 type

[0273] Figure 8 The produced battery is shown by a schematic expansion diagram. The positive electrode 23 is mixed with 10% by mass of sulfur (S8), 60% by mass of Ketjen black as a conductive aid, and 30% by mass of polytetrafluoroethylene (PTFE) as a binder using an agate mortar. And, while adapting it with acetone, it is rolled into shape using a roller press for about 10 times. Thereafter, it is dried in a vacuum dryer at 70°C for 12 hours. In this way, the positive electrode 23 can be obtained.

[0274] The gasket 22 was placed in the button battery can 21, and the positive electrode 23 made of sulfur, the separator 24 made of glass fiber, the negative electrode 25 made of a Mg plate with a diameter of 15 mm and a thickness of 200 μm, the spacer 26 made of a stainless steel plate with a thickness of 0.5 mm, and the button battery cover 27 were stacked in order, and then the button battery can 21 was sealed by riveting. The spacer 26 was spot welded to the button battery cover 27 in advance.

[0275] [3. Electrochemical measurement]

[0276] (Impedance measurement)

[0277] The battery produced as described above was used as an evaluation battery cell. The evaluation battery cell was placed in a thermostatic chamber and the impedance was measured under the following measurement conditions. The measurement was performed 3 hours after the thermostatic chamber reached each set temperature using a potentiostat (VMP3 manufactured by Bio-Logic).

[0278] Measurement conditions

[0279] Frequency: 1MHz~1Hz

[0280] Amplitude: 10mV

[0281] Temperature range: 25℃, 30℃~50℃ (every 10℃)

[0282] The resistance (unit: Ω) and ion conductivity (Mg ion conductivity) obtained at each temperature are shown in Table 1 and Fig.10 shown.

[0283] Table 1

[0284]

[0285] The Mg ion conductivity of the polymer solid electrolyte containing the Mg polymer salt (5-2) at 50°C is 1.3×10 -5 S / cm. In addition, it was confirmed that the Mg ion conductivity increases with the increase in temperature (temperature dependence). In contrast, in the inorganic solid electrolytes described in Patent Documents 1 and 2 as comparative examples, the ion conductivity at 500°C is 1.1×10 -9 ~about 3.6×10 -6 S / cm. The inorganic solid electrolyte also has the temperature dependence of ion conductivity like the above-mentioned polymer solid electrolyte, so it is expected that the ion conductivity at 50°C is much smaller than the ion conductivity at 500°C. Therefore, it can be seen that the polymer solid electrolyte of the embodiment has an ion conductivity at least 1 to 3 orders of magnitude greater than that of the inorganic solid electrolyte of the comparative example.

[0286] Summarizing the above, the following matters were found from this confirmation experiment.

[0287] The polymer solid electrolyte of the embodiment includes a Mg polymer salt (5-2). The Mg polymer salt (5-2) includes Mg 2+ and a Mg polymer salt of an anionic polymer having an anionic functional group and a coordinating functional group. Therefore, if a Mg polymer salt having such a composition and structure is included, it can contribute to higher Mg ion conductivity.

[0288] The Mg polymer salt (5-2) contained in the polymer solid electrolyte of the example has a coordinating substituent in the main chain. Therefore, if the Mg polymer salt having such a structure is contained, it can contribute to higher Mg ion conductivity.

[0289] The Mg polymer salt (5-2) contained in the polymer solid electrolyte of the example has poly(alkylene oxide) (more specifically, poly(ethylene oxide)) as a coordinating substituent in the main chain. Therefore, if a Mg polymer salt having such a structure is contained, it can contribute to higher Mg ion conductivity.

[0290] The Mg polymer salt (5-2) contained in the polymer solid electrolyte of the example has an anionic functional group (particularly a trifluoromethylsulfonamide group) in the side chain. Therefore, if a Mg polymer salt having such a structure is contained, it can contribute to higher Mg ion conductivity.

[0291] The polymer solid electrolyte of the example contains a Mg polymer salt and therefore has flexibility and can contribute to structural maintenance.

[0292] Industrial Applicability

[0293] The polymer solid electrolyte of the present invention can be used in various fields that utilize electrochemical reactions to extract energy. Although it is only illustrated, the polymer solid electrolyte of the present invention is of course not limited to secondary batteries, but can also be used in various electrochemical devices such as capacitors, air batteries, and fuel cells.

[0294] Explanation of symbols

[0295] 10. positive electrode; 11. negative electrode; 12. electrolyte layer; 31. positive electrode; 32. negative electrode; 33. diaphragm; 35, 36. current collector; 37. gasket; 41. porous positive electrode; 42. negative electrode; 43. diaphragm and solid electrolyte; 44. current collector on the air electrode side; 45. current collector on the negative electrode side; 46. diffusion layer; 47. oxygen selective permeable membrane; 48. outer packaging body; 51. air (atmosphere); 52. oxygen; 100. magnesium secondary battery; 111. electrode structure storage member (battery can); 112, 113. insulating plate; 114. battery cover; 115. safety valve mechanism; 1 15A, disc plate; 116, thermistor element (PTC element); 117, gasket; 118, center pin; 121, electrode structure; 122, positive electrode; 123, positive electrode lead; 124, negative electrode; 125, negative electrode lead; 126, separator; 200, outer packaging member; 201, close-fitting film; 221, electrode structure; 223, positive electrode lead; 225, negative electrode lead; 1001, battery cell (assembled battery); 1002, magnesium secondary battery; 1010, control unit; 1011, memory; 1012, voltage measuring unit; 1013, current measuring unit 1014, current detection resistor; 1015, temperature measurement unit; 1016, temperature detection element; 1020, switch control unit; 1021, switch unit; 1022, charge control switch; 1024, discharge control switch; 1023, 1025, diode; 1031, positive terminal; 1032, negative terminal; CO, DO, control signal; 2000, housing; 2001, control unit; 2002, various sensors; 2003, power supply; 2010, engine; 2011, generator; 2012, 2013, inverter; 2014, drive motor; 2015, differential device; 2016, transmission; 2017, clutch; 2021, front wheel drive shaft; 2022, front wheel; 2023, rear wheel drive shaft; 2024, rear wheel; 3000, house; 3001, control unit; 3002, power supply; 3003, smart meter; 3004, power hub; 3010, electrical equipment (electronic equipment); 3011, electric vehicle; 3021, generator for self-generation; 3022, centralized power system; 4000, tool body; 4001, control unit; 4002, power supply; 4003, drill head.

Claims

1. A polymer solid electrolyte for an electrochemical device having a magnesium electrode as a negative electrode, The polymer solid electrolyte is composed of a Mg polymer salt, wherein the Mg polymer salt contains Mg 2+ and an anionic polymer having an anionic functional group and a coordinating functional group, The polymer solid electrolyte has Mg ion conductivity, The anionic functional group is a trifluoromethylsulfonamide group.

2. The polymer solid electrolyte according to claim 1, wherein The anionic polymer has the anionic functional group in a side chain.

3. The polymer solid electrolyte according to claim 1 or 2, wherein: The anionic polymer has the coordinating functional group in the main chain.

4. The polymer solid electrolyte according to claim 1 or 2, wherein: The anionic polymer is a triblock copolymer represented by the general formula (1), (A)-(B)-(A) (1) In the general formula (1), (A) represents a block having an anionic functional group, and (B) represents a block having a coordinating functional group.

5. The polymer solid electrolyte according to claim 4, wherein In the general formula (1), (A) is a block represented by the general formula (2), In the general formula (2), Af represents an anionic functional group, m represents an integer of 3 to 40, and p represents an integer of 1 to 10.

6. The polymer solid electrolyte according to claim 4, wherein In the general formula (1), (B) is a block represented by the general formula (3), In the general formula (3), n represents an integer of 150-850, and q represents an integer of 1-10.

7. The polymer solid electrolyte according to claim 1 or 2, wherein: The coordinating functional group is poly(ethylene oxide).

8. The polymer solid electrolyte according to claim 1 or 2, wherein: The positive electrode of the electrochemical device is a sulfur electrode including sulfur.

9. A method for producing a polymer solid electrolyte, which is a method for producing a polymer solid electrolyte having Mg ion conductivity. The method for producing the polymer solid electrolyte comprises the following steps: The Li polymer salt represented by the general formula (4) is dissolved in a linear ether solution of a Mg salt, and a linear ether is added to precipitate a Mg polymer salt represented by the general formula (5). In the general formula (4), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same as or different from each other. In the general formula (5), Af represents an anionic functional group, T represents a terminal group, m represents an integer of 3 to 40, n represents an integer of 150 to 850, p and q represent integers of 1 to 10, and p and q may be the same as or different from each other.

10. The method for producing a polymer solid electrolyte according to claim 9, wherein: In the general formulae (4) and (5), the anionic functional group is a trifluoromethylsulfonamide group.

11. The method for producing a polymer solid electrolyte according to claim 9 or 10, wherein: In the general formulae (4) and (5), q represents 2.

12. An electrochemical device comprising a negative electrode and a positive electrode, The negative electrode is a magnesium electrode, The solid electrolyte of the electrochemical device is the polymer solid electrolyte according to any one of claims 1 to 8.

13. The electrochemical device according to claim 12, wherein: The positive electrode is a sulfur electrode including sulfur.

Citation Information

Patent Citations

  • Solid electrolyte having magnesium ion conductivity and magnesium secondary battery using the same

    US20180102567A1

  • Solid electrolyte having magnesium ion conductivity and magnesium secondary battery using the same

    US20180159170A1

  • Solid polymeric electrolytes based on triblock copolymers, in particular polystyrene-poly(oxyethylene)-polystyrene copolymers

    CN101466750A

  • Polymers based on ionic monomers, compositions comprising them, methods for their manufacture and their use in electrochemical applications

    CN115038738A