Flexible high-density scalp EEG electrode and preparation method thereof
By using PDMS, carbon conductive materials, titanium dioxide nanopowder and other components in scalp EEG electrodes to build a conductive mesh, and adding conductive liquid, the rigidity and impedance problems of scalp electrodes in the existing technology are solved, achieving high density, stability and comfort. EEG signal collection.
Patent Information
- Application Number
- CN202210909885.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-07-29
AI Technical Summary
The rigid materials of existing non-invasive high-density scalp EEG electrodes cannot fit tightly on the head, especially in developed areas, and can easily cause damage to the skin. The signal-to-noise ratio is low and the impedance is too large, which is not conducive to signal collection.
Polydimethylsiloxane (PDMS) is used as a flexible material, carbon conductive material and titanium dioxide nanopowder are added, and tetrachloroauric acid is used to reduce the gold nanoparticles to build a conductive network, which reduces the polarization potential and improves the conductivity. Through N The channel collects local high-density signals and is equipped with conductive liquid to adjust the impedance.
A scalp EEG electrode with stable signal, high density, flexibility and comfort has been realized, which improves the signal-to-noise ratio and collection efficiency, reduces the scalp interface impedance, and enhances the collection ability of EEG signals.
Smart Images

Figure CN116019455B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of scalp EEG electrodes, and in particular relates to a flexible high-density scalp EEG electrode and a preparation method thereof. Background Art
[0002] As the center of the nervous system, the brain is the most complex system in structure and function known to humans. Due to its important significance in the fields of life sciences, medical health, etc., humans have never stopped studying the brain. Collecting and analyzing the electrical signals generated in the brain is an effective means of studying the brain. The electrical signals in the brain can reflect a person's health and condition, and are important parameters for the treatment of brain diseases. Scalp EEG has attracted many scientists to explore because of its non-destructive, convenient and low-cost characteristics.
[0003] Electroencephalogram (EEG) is the most commonly used and economical non-invasive method of brain wave detection. EEG has a high temporal resolution and is of great value in the treatment of epilepsy and mental illness. EEG can be divided into scalp electrode EEG and intracranial electrode EEG according to whether the electrodes are placed inside or outside the skull. EEG is similar to electrocardiogram and electromyography. Figure 1 The scalp electrode electroencephalogram is a graph obtained by placing electrodes at specific locations on the scalp, collecting microvolt signals generated by synchronous neuronal activity in the brain, and then amplifying and recording them. It is the spontaneous and rhythmic electrical activity of brain cell groups recorded by electrodes.
[0004] With the continuous development of EEG applications, the requirements for EEG signal collection electrodes are getting higher and higher. Depending on whether the electrodes are invasive, they can be divided into two categories: non-invasive electrodes and invasive electrodes. Common non-invasive electrodes include scalp EEG recording electrodes (Ag / AgCl electrodes); invasive electrodes include metal microwire electrodes, glass microelectrodes, silicon-based microelectrodes, and cerebral cortex electrical signal recording electrodes. Invasive electrodes can cause damage to the subjects, so non-invasive electrodes are mostly used to collect EEG signals.
[0005] Non-invasive electrodes are divided into dry electrodes, wet electrodes and semi-dry electrodes, and they exist in various forms, including single-channel electrodes, high-density electrodes, brush-shaped semi-dry electrodes, etc. Since the brain may need to work together between different regions when it is stimulated by sensation or performs cognitive activities, the information of a single local area cannot describe the entire perception pattern. Therefore, it is necessary to expand the research from single-channel to multi-channel EEG signals. High-density electrodes came into being, which contain multiple channels, mainly to collect more independent and effective signals within a limited range of space. The more channels there are, the more information is obtained. High-density acquisition is of great significance for exploring the laws of potential changes in the brain, studying brain mechanisms and brain-computer interfaces. With the continuous deepening of research on high-density electrodes, fine movement control can be performed through the contraction movement of local brain channel areas and nerve-controlled muscle tissues. However, the rigid materials of existing non-invasive high-density electrodes cannot fit tightly to the head, especially in the hairy area, which is easy to damage the skin, and the low signal-to-noise ratio and excessive impedance are not conducive to signal acquisition. Summary of the invention
[0006] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a flexible high-density scalp EEG electrode, which uses polydimethylsiloxane (PDMS) as a flexible material, adds a carbon conductive material to construct a conductive network, then adds titanium dioxide nanopowder and tetrachloroauric acid, uses the advantage of a wide negative potential window of titanium dioxide nanopowder to reduce polarization potential and improve scalp affinity, uses tetrachloroauric acid reduction to provide gold nanoparticles to improve conductivity and electron capture ability, and performs local high-density signal acquisition through an N channel. The flexible high-density scalp EEG electrode of the present invention has the advantages of stable signal, high density, flexibility, and comfort.
[0007] Another object of the present invention is to provide a method for preparing the above-mentioned flexible high-density scalp EEG electrode.
[0008] Another object of the present invention is to provide a conductive liquid, which can quickly adjust the impedance to a stable state when combined with a flexible high-density scalp EEG electrode.
[0009] The purpose of the present invention is achieved through the following technical solutions.
[0010] A flexible high-density scalp EEG electrode, comprising: a carrier and N tantalum wires, wherein the carrier comprises: a base and N claw posts connected to the bottom surface of the base, each claw post passes through one tantalum wire, wherein the bottom end of each tantalum wire is flush with the bottom surface of the claw post, and is used to collect ions to form a microcurrent, and the top end of the tantalum wire is located above the base, and is used to connect with the electrode wire, wherein the carrier is solidified by a sensitive material, and the method for preparing the sensitive material is: PDMS is uniformly mixed with a tetrachloroauric acid aqueous solution, and then The temperature is kept at 70-80° C. for 1-1.5 h to reduce the tetrachloroauric acid to gold particles or gold trichloride, and then cooled to room temperature. A hybrid is added and ultrasonicated to obtain a sensitive material, wherein the hybrid is a mixture of a carbon conductive material and titanium dioxide nanopowder. The mass ratio of tetrachloroauric acid, carbon conductive material, titanium dioxide nanopowder and PDMS in the tetrachloroauric acid aqueous solution is (0.000003-0.000006):(0.5-3):(0.5-2.5):(92-99) by mass.
[0011] In the above technical solution, the PDMS is formed by mixing a silicone elastomer base and a silicone elastomer curing agent, and the ratio of the silicone elastomer base to the silicone elastomer curing agent is (9-11):1 in terms of mass fraction.
[0012] In the above technical solution, the carbon conductive material is a multi-walled carbon nanotube or a single-walled carbon nanotube.
[0013] In the above technical solution, the concentration of tetrachloroauric acid in the tetrachloroauric acid aqueous solution is 10 -6 ~10 -4 mol / L.
[0014] In the above technical solution, N=19.
[0015] In the above technical solution, the length of the tantalum wire is 5 to 6 cm, the diameter of the tantalum wire is 0.2 to 0.6 mm, the claw column is a truncated cone that tapers from top to bottom, the height of the claw column is 3 to 6 mm, the diameter of the bottom circle of the claw column is 1 to 1.5 mm, the diameter of the top circle of the claw column is 2 to 2.5 mm, the axial center distance between adjacent claw columns is 2.5 to 4 mm, the base is cylindrical, the diameter of the base is 15 to 20 mm, and the height of the base is 6 to 10 mm.
[0016] The method for preparing the above-mentioned flexible high-density scalp EEG electrode comprises the following steps:
[0017] 1) Pour the sensitive material into the mold twice, and maintain the vacuum for 10 to 15 minutes after each pouring;
[0018] In the step 1), the pressure is evacuated to below -0.08 MPa.
[0019] In the step 1), the mass ratio of the sensitive material poured into the mold in two batches is (2-3):5.
[0020] 2) inserting N tantalum wires into the sensitive material and maintaining the temperature at 60-80° C. for 2-5 hours to solidify the sensitive material to form the carrier, and taking out the flexible high-density scalp EEG electrode from the mold.
[0021] A conductive liquid is prepared by mixing sodium carboxymethyl cellulose (CMC) and saturated saline solution, wherein the ratio of the mass fraction of the sodium carboxymethyl cellulose to the volume fraction of the saturated saline solution at 25°C is (1-1.1):20, the unit of the mass fraction is g, and the unit of the volume fraction is mL.
[0022] In the above technical solution, the conductive liquid is used in conjunction with flexible high-density scalp EEG electrodes.
[0023] The beneficial effects of the present invention are as follows:
[0024] 1. The sensitive material of the present invention is based on polydimethylsiloxane, has good flexibility, and will not cause discomfort to the subjects;
[0025] 2. The titanium dioxide nanopowder used in the sensitive material of the present invention has excellent chemical stability, thermal stability and antibacterial properties; the tetrachloroauric acid gradually reduces the gold particles during the two heating processes, thereby improving the electron capture ability of the sensitive material;
[0026] 3. The flexible high-density scalp EEG electrode makes the collection of EEG signals in the hairline area more stable, convenient and fast due to its high density and conductive liquid;
[0027] 4. The circuit adopts N-lead mode to reduce the scalp interface impedance. Due to its special structure, the carrier behaves as an insulator when not powered, and behaves as a conductor with low impedance when powered. The performance advantage is obvious and has a high correlation with the traditional wet electrode.
[0028] 5. The conductive liquid is in a paste-like state and is not easy to flow. During the test, it can adhere well to the flexible high-density scalp EEG electrodes, which is convenient for the testing of EEG signals. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a photo of the flexible high-density scalp EEG electrode of the present invention;
[0030] Figure 2 is a bottom view of the carrier (numbered);
[0031] Figure 3 This is a cross-sectional view of a flexible high-density scalp EEG electrode;
[0032] Figure 4This is a photo of the flexible high-density scalp EEG electrode test (above the brow bone);
[0033] Figure 5 The impedance of the traditional wet electrode-Ag / AgCl electrode and the flexible high-density scalp EEG electrode;
[0034] Figure 6 It is the original signal waveform (blink), and the concave part is the blink waveform;
[0035] Figure 7 It is the original signal waveform (grinding teeth), and the sawtooth shape is the gnashing teeth waveform;
[0036] Figure 8 It is the correlation between the eye-blinking signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode;
[0037] Fig. 9 It is the correlation between the teeth biting signal of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode;
[0038] Fig.10 This is a photo of the flexible high-density scalp EEG electrode test (occipital area);
[0039] Fig.11 The impedance of the traditional wet electrode-Ag / AgCl electrode and the flexible high-density scalp EEG electrode;
[0040] Fig.12 is the original signal waveform (eyes open and closed);
[0041] Fig.13 It is the correlation between the eye opening and closing signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode;
[0042] Fig.14 This is the signal-to-noise ratio diagram of each antenna of the flexible high-density scalp EEG electrode (the "I"-shaped line in the figure is the error bar);
[0043] Fig.15 The spectrum of the flexible high-density scalp EEG electrode with the eyes closed and open is shown in Figure 1. XC represents the spectrum in the eyes-closed state (the more convex line in the figure), and XO represents the spectrum in the eyes-open state (the more gentle line in the figure). X = integers from 1 to 19, representing Figure 2 Antennae numbered 1 to 19;
[0044] Fig.16 The correlation between the eye opening and closing signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode in Example 2;
[0045] Fig.17is the signal-to-noise ratio of each antenna of the flexible high-density scalp EEG electrode in Example 2 (the "I"-shaped line in the figure is the error bar);
[0046] Fig.18 The spectrum of the flexible high-density scalp EEG electrode in Example 2 when the subject has eyes closed and eyes open, XC represents the spectrum in the eyes closed state (the more convex line in the figure), XO represents the spectrum in the eyes open state (the more gentle line in the figure), X=an integer in the range of 1 to 19, representing Figure 2 Antennae numbered 1 to 19;
[0047] Fig.19 is the correlation between the antennae of the flexible high-density scalp EEG electrode;
[0048] Fig. 20 The interface contact impedances of the planar electrode prepared from the sensitive material obtained in Example 1 and the planar electrode prepared from the sensitive material obtained in Comparative Example 1 and the saturated sodium chloride aqueous solution, respectively;
[0049] Fig.21 The following are curved photographs of thin sheets cured from the sensitive materials in Example 1 and Comparative Example 1;
[0050] Fig. 22 This is a photo of the discs being put into the roller machine and extruded separately. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0052] The sources of the drugs involved in the following embodiments are as follows:
[0053] 1. Multi-walled carbon nanotubes, manufacturer: Shenzhen Turing Evolution Technology Co., Ltd.;
[0054] 2. Single-walled carbon nanotubes, manufacturer: Nanjing Xianfeng Nanomaterial Technology Co., Ltd.;
[0055] 3. Titanium dioxide nanopowder, manufacturer: Siping Gaosida Nanomaterial Equipment Co., Ltd.;
[0056] 4. Tetrachloroauric acid, manufacturer: Alfa Aesar (USA);
[0057] 5. Sodium carboxymethyl cellulose, manufacturer: Tianjin Xingfu Fine Chemical Research Institute;
[0058] 6. Silicone elastomer substrate and silicone elastomer curing agent were purchased from Dow Corning PDMS, model: 184;
[0059] 7. Conductive paste, manufacturer: Compumedics (USA);
[0060] The sources of the instruments involved in the following embodiments are as follows:
[0061] 1. Vacuum drying oven: Product model: DZF-6050, manufacturer: Shanghai Yiheng Scientific Instrument Co., Ltd.;
[0062] 2. Constant temperature magnetic stirrer: product model B11-2, manufacturer: Shanghai Si Le Instrument Co., Ltd.;
[0063] 3. Ultrasonic cleaner: product model: KQ2200E.
[0064] The preparation method of tetrachloroauric acid aqueous solution is as follows: first, place a 25mL beaker on a balance and zero it, then quickly weigh 0.3397g of tetrachloroauric acid with a spoon, pour it into a 10mL volumetric flask, add anhydrous ethanol to make up the volume, obtain a 0.1mol / L tetrachloroauric acid aqueous solution, and dilute to 10 -4 mol / L.
[0065] Before use, the tantalum wire was polished with 220-mesh (68 μm) fine sandpaper to remove surface oxides and dirt, and then ultrasonically cleaned in 99.7 wt % alcohol and ultrapure water for 5 min each, and dried naturally.
[0066] The conductive liquid in the following embodiment is prepared by mixing sodium carboxymethyl cellulose (CMC) and 25°C saturated salt water, the mass fraction of sodium carboxymethyl cellulose and the volume fraction of saturated salt water is 1.1:20, the unit of mass fraction is g, and the unit of volume fraction is mL. Preparation of conductive liquid: Weigh sodium carboxymethyl cellulose (CMC) with an electronic balance and pour it into a beaker, then add saturated salt water, stir evenly, add a rotor and place it on a magnetic stirrer at 80r / s for 5 hours.
[0067] Example 1
[0068] like Figure 1 As shown, a flexible high-density scalp EEG electrode includes: a carrier and N tantalum wires, the carrier includes: a substrate and N claw posts connected to the bottom surface of the substrate, N=19, and the arrangement of the N claw posts is as follows Figure 2 As shown, N claw posts are divided into six rows, and the number of claw posts in each row from top to bottom is: 3, 4, 5, 4 and 3, and the claw posts in adjacent rows are staggered. Figure 3 As shown, each claw column passes through a tantalum wire, wherein the bottom end of each tantalum wire is flush with the bottom surface of the claw column, and is used to collect ions to form a microcurrent. The top end of the tantalum wire is located above the substrate and is used to connect with the electrode wire. One tantalum wire is connected to one electrode wire. The N electrode wires are numbered and connected to the signal acquisition device, and the numbering is as follows: Figure 2As shown, the carrier is solidified by the sensitive material, and the method for preparing the sensitive material is: PDMS and tetrachloroauric acid aqueous solution are mixed evenly, kept at 78°C for 1.5h, cooled to room temperature 20-25°C, tetrachloroauric acid is reduced to gold particles or gold trichloride, a hybrid is added, and ultrasonication is performed for 5min to obtain the sensitive material, wherein the hybrid is a mixture of carbon conductive material and titanium dioxide nanopowder, and the mass ratio of tetrachloroauric acid, carbon conductive material, titanium dioxide nanopowder and PDMS in the tetrachloroauric acid aqueous solution is 0.000003:1.7:2.1:96.17 by mass.
[0069] PDMS is made of a mixture of a silicone elastomer base and a silicone elastomer curing agent. The ratio of the silicone elastomer base to the silicone elastomer curing agent is 10:1 by weight. The carbon conductive material is multi-walled carbon nanotubes. The concentration of tetrachloroauric acid in the tetrachloroauric acid aqueous solution is 10 -4 mol / L.
[0070] The length of the tantalum wire is 5 cm, and the diameter of the tantalum wire is 0.2 mm; the claw column is a truncated cone that tapers from top to bottom, the height of the claw column is 6 mm, the diameter of the bottom circle of the claw column is 1.5 mm, the diameter of the top circle of the claw column is 2.5 mm, the axial center distance between adjacent claw columns is 3.5 mm, the base is cylindrical, the diameter of the base is 20 mm, and the height of the base is 10 mm.
[0071] The method for preparing the above-mentioned flexible high-density scalp EEG electrode comprises the following steps:
[0072] 1) Pour the sensitive material into the mold twice, with the mass ratio of the sensitive materials poured into the mold successively being 2:5. After each pouring, evacuate to -0.08Mpa and maintain for 10 minutes;
[0073] 2) N tantalum wires were inserted into the sensitive material and kept at a constant temperature of 72° C. for 2 h to solidify the sensitive material to form a carrier, and the flexible high-density scalp EEG electrode was taken out from the mold.
[0074] The above-mentioned flexible high-density scalp EEG electrodes were used for testing: three traditional wet electrodes - Ag / AgCl electrodes (produced by Beijing Qingjing Electronic Technology Co., Ltd.), scrub, conductive paste, dust-free cloth, medical tape and conductive liquid were prepared, and the equipment used for signal acquisition was the Greal model 32-lead EEG acquisition device from the Australian Neuroscan company.
[0075] (1) Collection of EEG signals of blinking and clenching teeth in the hairless area
[0076] The impedance and signal waveform of the flexible high-density scalp EEG electrode are observed and the correlation between electrodes is analyzed by using the traditional wet electrode-Ag / AgCl electrode as a reference. First, wipe the mastoid behind the ear of the subject with a small amount of scrub with a dust-free cloth. The function of the scrub is to remove the stratum corneum on the surface of the mastoid. Apply 0.2mL of conductive paste on each of the two traditional wet electrode-Ag / AgCl electrodes to fill the concave part of the traditional wet electrode-Ag / AgCl electrode. Then use medical tape to fix them at the two mastoid positions behind the ear, one of which is used as a reference electrode and the other as a ground electrode. Select two adjacent positions above the subject's brow bone and wipe them with scrub as area one and area two. Apply an equal amount of conductive paste on the third traditional wet electrode-Ag / AgCl electrode and place it in area one. Apply the flexible high-density scalp EEG electrode with conductive liquid and place it in area two. Fix it with a headband, as shown in the figure. Figure 4 As shown. Tested with Grael EEG equipment and Curry 8 software. Each tantalum wire of the flexible high-density scalp EEG electrode has a tentacles at one end that contacts the skin, and the tentacles are independently connected to the Greal EEG equipment. The impedance value is as follows Figure 5 As shown in the figure, 1 to 19 represent the N antennae of the flexible high-density scalp EEG electrode, and 27 represents the traditional wet electrode-Ag / AgCl electrode; the original waveform of the blink is shown in Figure 6 As shown, the original waveform of biting teeth is as follows Figure 7 As shown in the figure, under the premise that the contact area between each antenna of the flexible high-density scalp EEG electrode and the scalp is less than 3% of the contact area between the traditional wet electrode-Ag / AgCl electrode and the scalp, the impedance of each antenna of the flexible high-density scalp EEG electrode is close to the impedance of the traditional wet electrode-Ag / AgCl electrode.
[0077] The EEG signals collected by the flexible high-density scalp EEG electrodes were processed using MATLAB, and then the Origin2018 software was used to draw the graph. The correlation between the blinking signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode was about 97%. Figure 8 As shown in the figure, the correlation between the teeth biting signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode is about 97%. Fig. 9 shown.
[0078] (2) EEG signal collection of eyes open and closed in the occipital area
[0079] First, wipe the subject's mastoid process behind the ear with a dust-free cloth and a small amount of scrub. Apply conductive paste on the two traditional wet electrode-Ag / AgCl electrodes to fill the wet electrode-Ag / AgCl electrode concave, and then fix them at the two mastoid positions behind the ear with medical tape, one of which is used as a reference electrode and the other as a ground electrode. Select two adjacent locations in the subject's occipital area and wipe them with scrub as area one and area two. Apply the same amount of conductive paste on the third traditional wet electrode-Ag / AgCl electrode and place it in area one. Dip the flexible high-density scalp EEG electrode in conductive liquid and place it in area two and fix it with a headband. The traditional wet electrode-Ag / AgCl electrode is about 3 cm above the flexible high-density scalp EEG electrode and fixed with a head net. Wear as shown in the figure Fig.10 shown.
[0080] During the test, a conductive liquid was applied to the bottom of the claw column, and the impedance of each channel of the flexible high-density scalp EEG electrode was reduced to about 30kΩ~50kΩ by slightly adjusting the distance between the scalp and the bottom of the claw column. After the impedance value was relatively stable, the signal was collected. The adjustment time was within half an hour. Fig.11 As shown in the figure, 1 to 19 represent the N antennae of the flexible high-density scalp EEG electrode, and 27 represents the traditional wet electrode-Ag / AgCl electrode. The original waveform of opening and closing the eyes is as follows Fig.12 As shown, Fig.12 The left side of the middle vertical line is the subject's eyes closed state (right side is the eyes open state), the waveform amplitude is large and sparse, and alpha waves appear at this time. The collected EEG signals were processed with MATLAB and then plotted with Origin. The correlation between the open and closed eye signals of each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode can reach 98%, such as Fig.13 As shown in the figure. The signal-to-noise ratio of each antenna of the flexible high-density scalp EEG electrode can reach about 7.6dB. Fig.14 shown.
[0081] The subjects were asked to keep their eyes closed or open. The EEG signals collected under the eyes closed and eyes open were processed by Origin 2018 software to convert the time domain to frequency domain. The spectrum of each antenna of the flexible high-density scalp EEG electrode is shown in the figure. Fig.15 When a person is awake, eyes closed, and quiet, they will produce an alpha rhythm of 8 to 13 Hz, such as Fig.15 As shown in the peak value in , the amplitude of the alpha wave rhythm can be used as a criterion for measuring the quality of EEG electrodes. Fig.15 It can be obtained that the alpha wave amplitude measured by the flexible high-density scalp EEG electrodes of the subjects with their eyes closed is around 6μV.
[0082] In the above test, if the conductive liquid is not applied to the bottom of the claw post, the impedance of the flexible high-density scalp EEG electrode is greater than 250kΩ and signal collection cannot be performed. If physiological saline is applied to the bottom of the claw post, the impedance will also decrease, but the fluidity of physiological saline is strong, which makes it inconvenient to collect EEG signals. If conductive paste is applied to the bottom of the claw post, although the final impedance value can also be reduced to 30kΩ~50kΩ, the impedance reduction time is slower, about 40 minutes.
[0083] Comparative Example 1
[0084] A flexible comb-shaped semi-dry electrode is the flexible comb-shaped semi-dry electrode disclosed in Example 3 of the specification in publication number CN112967832A.
[0085] The flexible high-density scalp EEG electrode obtained in Example 1 and the flexible comb-shaped semi-dry electrode obtained in Comparative Example 1 were compared.
[0086] The flexible comb-shaped semi-dry electrode has a large area of contact between the bottom surfaces of the 19 claws and the skin. The impedance obtained by the bottom surfaces of the 19 claws is about 5 to 10 kΩ, and the resistance per square centimeter is calculated to be about 14 kΩ; the contact area between the bottom surface of each claw of the flexible high-density scalp EEG electrode and the skin is less than three percent of the contact area between the flexible comb-shaped electrode and the skin, the average impedance of the flexible high-density scalp EEG electrode is about 30 kΩ, and the resistance per square centimeter of the bottom surface of each claw of the flexible high-density scalp EEG electrode is about 4.7 kΩ; it can be seen that the sensitive material in Example 1 has the technical effect of reducing resistance compared with the sensitive material in Comparative Example 1.
[0087] The correlation between the flexible comb-shaped semi-dry electrode obtained in Comparative Example 1 and the traditional wet electrode-Ag / AgCl electrode is about 98%; the correlation between the antennae of the flexible high-density scalp EEG electrode obtained in Example 1 and the traditional wet electrode-Ag / AgCl electrode is also about 98%. The collected signals are processed by MATLAB and then plotted by Origin 2018 to obtain a correlation between the antennae of the flexible high-density scalp EEG electrode as high as 99%. Fig.19 shown.
[0088] The sensitive material in Example 1 and the sensitive material in Example 2 in CN112967832A are respectively made into planar electrodes, the planar electrodes comprising: a fan-shaped column formed by curing the sensitive material at 72°C for 2h, a tantalum wire with a diameter of 0.6mm is inserted into the sensitive material before curing, the thickness of the fan-shaped column is 3mm, the fan-shaped radius of the fan-shaped column is 10mm, the central angle of the fan-shaped column is 90°, the length of the tantalum wire is 5cm, one end of the tantalum wire is bent into a circle with a diameter of 2.2mm, and then the end of the tantalum wire with the circle is inserted into the fan-shaped column. The planar electrode made of the sensitive material in Example 1 is Au-TiO2-CNT@PDMS, and the planar electrode made of the sensitive material in Example 2 in CN112967832A is Cu-TiO2-CNT@PDMS.
[0089] The contact impedance of Au-TiO2-CNT@PDMS and Cu-TiO2-CNT@PDMS with 25°C saturated sodium chloride aqueous solution was tested by electrochemical workstation and three-electrode system. The three-electrode system is composed of counter electrode, reference electrode and working electrode, where the counter electrode is a platinum sheet electrode, the reference electrode is a silver-silver chloride electrode, and the working electrode is a flat electrode. The three-electrode system is immersed in 25°C saturated sodium chloride aqueous solution. The test results are as follows: Fig. 20 As shown. Fig. 20 It can be seen that the interfacial contact impedance of the working electrode prepared from the sensitive material obtained in Example 1 is smaller than the interfacial contact impedance of the working electrode prepared from the sensitive material obtained in Example 2 in CN112967832A.
[0090] The sensitive materials in Example 1 and Comparative Example 1 were cured at 72°C for 2 hours to form thin sheets with a length of 1 cm, a width of 5 mm, and a thickness of 1 mm. The bending degree was observed. Fig.21 As shown in the figure, the left side is the sensitive material in Example 1, and the right side is the sensitive material in Comparative Example 1. It can be seen from the figure that the bending degree of the sensitive material in Example 1 is smoother.
[0091] The sensitive materials in Example 1 and Comparative Example 1 were cured at 72°C for 2 hours to form discs with a diameter of 20 mm and a thickness of 3 mm, and their deformation degree was tested by a roller machine. The roller gap of the roller machine was set to 1 mm, and the disc was placed in it to test its thickness and recovery time after extrusion.
[0092] Place the disc into the roller machine, such as Fig. 22As shown. Deformed during extrusion, recovered after extrusion. The disc was put into the roller machine and extruded for 1min, 5min, 10min, 30min, and 1h respectively, and then taken out. When the extrusion time was 1 to 30min, there was no obvious change in the disc after extrusion. When the extrusion time was 1h, the thickness of the disc made of the sensitive material in Comparative Example 1 changed from 3mm to 2.91mm, and recovered to 3mm after 30s, while the disc made of the sensitive material in Example 1 had no obvious change.
[0093] The sectors with 1 / 4 area of each of the two discs were extruded in a roller mill for multiple times, each extrusion lasting 5 seconds. The sectors obtained from the sensitive material in Example 1 had cracks at the 15th extrusion, and the sectors obtained from the sensitive material in Comparative Example 1 had cracks at the 6th extrusion.
[0094] Example 2
[0095] A flexible high-density scalp EEG electrode is basically the same as that of Example 1, except that the carbon conductive material is a single-walled carbon nanotube.
[0096] The collected eye opening and closing signals were processed and plotted. The signal correlation between each antenna of the flexible high-density scalp EEG electrode and the traditional wet electrode-Ag / AgCl electrode is shown in the figure. Fig.16 As shown, the signal-to-noise ratio Fig.17 As shown, the spectrum diagram is Fig.18 shown.
[0097] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.
Claims
1. A flexible high-density scalp EEG electrode, characterized in that: include: A carrier and N tantalum wires, wherein the carrier comprises: a substrate and N claw posts connected to the bottom surface of the substrate, each claw post passes through one tantalum wire, wherein the bottom end of each tantalum wire is flush with the bottom surface of the claw post, and is used to collect ions to form a microcurrent, and the top end of the tantalum wire is located above the substrate, and is used to connect with the electrode wire, wherein the carrier is solidified by a sensitive material, and the method for preparing the sensitive material is: PDMS and a tetrachloroauric acid aqueous solution are mixed evenly, and kept at 70 to 80°C for 1 to 1.5 hours, so that the tetrachloroauric acid Acid reduction to gold particles or gold trichloride, cooling to room temperature, adding a hybrid, ultrasonication, to obtain a sensitive material, wherein the hybrid is a mixture of a carbon conductive material and titanium dioxide nanopowder, and the mass ratio of tetrachloroauric acid, carbon conductive material, titanium dioxide nanopowder and PDMS in the tetrachloroauric acid aqueous solution is (0.000003-0.000006):(0.5-3):(0.5-2.5):(92-99) by weight, and the concentration of tetrachloroauric acid in the tetrachloroauric acid aqueous solution is 10 -6 ~10 -4 mol / L, the PDMS is formed by mixing a silicone elastomer base and a silicone elastomer curing agent, and the ratio of the silicone elastomer base to the silicone elastomer curing agent is (9-11):1 in parts by mass.
2. The flexible high-density scalp EEG electrode according to claim 1, characterized in that: The carbon conductive material is a multi-walled carbon nanotube or a single-walled carbon nanotube.
3. The flexible high-density scalp EEG electrode according to claim 1, characterized in that: The length of the tantalum wire is 5 to 6 cm, and the diameter of the tantalum wire is 0.2 to 0.6 mm.
4. The flexible high-density scalp EEG electrode according to claim 1, characterized in that: The claw column is a truncated cone that tapers from top to bottom, the height of the claw column is 3-6 mm, the diameter of the circular bottom surface of the claw column is 1-1.5 mm, the diameter of the circular top surface of the claw column is 2-2.5 mm, and the axial center distance between adjacent claw columns is 2.5-4 mm.
5. The flexible high-density scalp EEG electrode according to claim 1, characterized in that: The base is cylindrical, the diameter of the base is 15-20 mm, and the height of the base is 6-10 mm.
6. The method for preparing the flexible high-density scalp EEG electrode according to claim 1, characterized in that: The following steps are involved: 1) Pour the sensitive material into the mold twice, and maintain the vacuum for 10 to 15 minutes after each pouring; 2) inserting N tantalum wires into the sensitive material and maintaining the temperature at 60-80° C. for 2-5 hours to solidify the sensitive material to form the carrier, and taking out the flexible high-density scalp EEG electrode from the mold.
7. The preparation method according to claim 6, characterized in that: In the step 1), the pressure is evacuated to below -0.08 MPa.
8. The preparation method according to claim 6, characterized in that: In the step 1), the mass ratio of the sensitive material poured into the mold in two batches is (2-3):5.
Citation Information
Patent Citations
Electric conduction paste and preparation method thereof
CN107184995A
Flexible piezoresistive sensor and application thereof
CN112086553A
Flexible comb-shaped semi-dry electrode and preparation method thereof
CN112967832A