A method for one-step synthesis of single-atom metal catalysts by photocatalytic coordination anchoring

The single-atom metal catalyst is constructed in situ on the carrier through the photocatalytic coordination anchoring method, which solves the problems of complex preparation, high cost and low performance in the existing technology, realizes the preparation of efficient and environmentally friendly single-atom catalyst, and significantly improves the catalytic performance. , suitable for large-scale industrial production.

CN116020450BActive Publication Date: 2024-10-29SHANGHAI NORMAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211650834.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-10-29
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The existing single-atom catalyst preparation methods are complex, costly, and not environmentally friendly, and metal atoms are easily buried during the preparation process, resulting in a decrease in catalytic performance.

Method used

The photocatalytic coordination anchoring method is used to construct vacancies and N atom coordination sites in situ on the carrier to anchor single-atom metals. The metal precursor reacts with nitrile compounds through light irradiation to inhibit the formation of nanoparticles and prepare efficient single-atom metals. Atomic catalyst.

Benefits of technology

A simple and green single-atom catalyst preparation has been achieved. The catalytic performance is better than that of commercial catalysts and is suitable for large-scale industrial production. The reaction conditions are mild, low-toxicity, energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004010532730000011
    Figure HDA0004010532730000011
  • Figure HDA0004010532730000012
    Figure HDA0004010532730000012
  • Figure HDA0004010532730000021
    Figure HDA0004010532730000021
Patent Text Reader

Abstract

The present invention discloses a method for synthesizing a single-atom metal catalyst by photocatalytic coordination anchoring in one step, and belongs to the technical field of catalyst preparation. The method comprises the following steps: dispersing a metal precursor solution into a mixed solution of a nitrile compound containing a photocatalyst, and preparing a single-atom catalyst by light irradiation. The photochemical method of the present invention has a wide range of applications and can be used to synthesize a variety of single-atom catalyst materials, and the catalyst has excellent catalytic performance. The photochemical reduction method used in the present invention has mild conditions and low toxicity of the reaction solution. This process has the advantages of being mild, energy-saving, green, environmentally friendly, low cost, and easy to operate, and is suitable for large-scale industrial preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a method for synthesizing a single-atom metal catalyst by photocatalytic coordination anchoring in one step. Background Art

[0002] Single-atom catalysts (SACs) have become one of the frontiers of research in heterogeneous catalysis. Compared with clusters or nanoparticles, isolated metal atoms in SACs have unconventional physicochemical properties, including unique electronic structures, maximized atomic utilization efficiency, unsaturated coordination environments, and strong metal-support interactions. These unique properties of SACs have opened up tremendous opportunities for applications in various catalytic fields and significantly improved their catalytic performance, such as thermal catalysis (e.g., CO / methane oxidation or hydrogenation), electrocatalysis (e.g., hydrogen production), and photocatalysis (e.g., CO2 reduction).

[0003] At present, the preparation of single-atom catalysts mainly includes atomic layer deposition (ALD), coprecipitation, metal organic framework carbonization, etc. In the atomic layer deposition (ALD) method, the support is alternately contacted with pulse vapor of metal precursors and O2. The number of pulse cycles must be carefully evaluated because when the metal precursor is further introduced, it may attach to the existing single metal species to form metal clusters. This method not only requires expensive experimental equipment, but also requires strict control of reaction parameters such as temperature and time. The coprecipitation method was first reported to synthesize Pt1 / FeOx SAC by adding a mixture of H2PtCl6 and Fe(NO3)3 solution to a Na2CO3 aqueous solution and then activating the filtrate. Many preparation parameters, such as the addition rate of the precursor solution, stirring speed, pH value, etc., will affect the performance of the final catalyst. In addition, during the preparation of single-atom catalysts by coprecipitation, some metal atoms will be buried at the support aggregation interface or encapsulated in the support. These buried single metal atoms cannot contact the reaction molecules to participate in the reaction, thus greatly reducing the performance of the single-atom catalyst. In the metal organic framework carbonization method, the precursor needs to be prepared using expensive reagents, and the types of metals prepared are relatively limited. This method is costly and the metal organic framework materials formed are poorly stable. Although there are many synthesis methods for SASC, most of the preparation methods are very complicated. The cumbersome procedures and specific conditions make the synthesis neither economical nor environmentally friendly. Therefore, it is urgent to develop a green and simple method for preparing single atom catalysts. Summary of the invention

[0004] In view of the defects of the prior art, the present invention proposes a simple and environmentally friendly photocatalytic coordination anchoring method, by in situ constructing vacancies (V o) and N atom coordination sites to anchor single atoms, while the oxidative free radicals generated in situ inhibit the formation of nanoparticles. The method is simple in steps, green and environmentally friendly, easy to achieve large-scale industrial production, and the catalytic performance of the prepared single atom catalyst is far superior to that of commercial catalysts.

[0005] In order to achieve the above object, the present invention provides a method for synthesizing a metal single-atom catalyst by photocatalytic coordination anchoring in one step, comprising the following steps:

[0006] Adding metal precursor and photocatalyst powder into nitrile compound and stirring thoroughly;

[0007] Light irradiation anchors the single atoms on the surface of the photocatalyst;

[0008] After the reaction is completed, the solid product is taken out, washed and dried to obtain a single atom catalyst.

[0009] Furthermore, the metal contained in the metal precursor includes precious metals or common metals; the precious metal includes one or more of ruthenium, rhodium, iridium, gold, silver, platinum or palladium, and the common metal includes one or more of iron, manganese, chromium, zinc, tin, lead, aluminum, copper, nickel or cobalt.

[0010] Furthermore, the metal precursor is a metal halide, preferably a metal chloride.

[0011] Furthermore, the nitrile compound includes one or more of acrylonitrile, acetonitrile, benzyl cyanide, cyanoacetic acid, malononitrile, cyanobenzyl or trimeramide.

[0012] Furthermore, the photocatalyst includes organic photocatalyst, inorganic photocatalyst and composite semiconductor photocatalytic material.

[0013] Furthermore, the organic photocatalyst includes carbon nitride and an organic porphyrin compound;

[0014] The inorganic photocatalyst includes titanium dioxide, bismuth oxyhalide and cadmium sulfide;

[0015] The composite semiconductor photocatalytic material comprises porphyrin-sensitized titanium dioxide, carbon nitride-loaded oxyhalogen bismuth, and carbon dot-modified titanium dioxide.

[0016] Furthermore, the dosage ratio of the photocatalyst to the nitrile compound is (0.25-4) mg / mL; and the dosage ratio of the metal element to the nitrile compound in the metal precursor is 0.1-1 mol / L.

[0017] Furthermore, the wavelength of the light irradiation is 150-1500nm, covering deep ultraviolet light, ultraviolet light, visible light and near infrared light; the illumination time is 4-8h.

[0018] The present invention also provides a single atom catalyst prepared according to the above method.

[0019] Furthermore, in the single-atom catalyst, the loading amount of metal single atoms is 0.01% to 5%, with the photocatalyst as the carrier.

[0020] Beneficial effects of the present invention:

[0021] 1. The photochemical coordination anchoring method used in the present invention has mild conditions and low toxicity of the reaction solution. This process has the advantages of being mild, energy-saving, green, environmentally friendly, low cost, and easy to operate, and is suitable for large-scale industrial preparation.

[0022] 2. The photochemical oxidation method used in the present invention is to construct V in situ on the carrier o The N atom coordination sites de-anchor the single atoms, while the in-situ generated oxidative free radicals inhibit the formation of nanoparticles.

[0023] 3. The photochemical method of the present invention has a wide range of applications and can be used to synthesize a variety of single-atom catalyst materials, and the catalyst has very excellent catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the XAFS graph of the single-atom catalyst material prepared in Example 1 of the present invention.

[0025] Figure 2 This is the HAADF-STEM image of the palladium single-atom catalyst material prepared in Example 1 of the present invention.

[0026] Figure 3 This is a comparison chart of the Suzuki cross-coupling reaction activities catalyzed by the Pd single atom catalyst prepared in Example 1 of the present invention, the Pd nanoparticle catalyst, and the commercial Pd / C. DETAILED DESCRIPTION

[0027] Example 1

[0028] Palladium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial anatase titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the solid catalyst was filtered and washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0029] Figure 1 This is the XAFS graph of the prepared Pd / TiO2 single atom catalyst material. The XAFS spectrum shows that no nanoparticles are formed in the Pd / TiO2 single atom catalyst.

[0030] Figure 2 This is the HAADF-STEM image of the prepared Pd / TiO2 single-atom catalyst material. The HAADF-STEM image shows that there are isolated Pd atoms in the Pd / TiO2 single-atom catalyst.

[0031] Figure 3 This is the activity diagram of the Suzuki cross-coupling reaction catalyzed by different catalysts. It can be seen that the catalytic performance of the Pd / TiO2 single atom catalyst is much higher than that of the Pd / TiO2 nanoparticle catalyst and the commercial Pd / C. The catalytic activity of the Pd / TiO2 single atom catalyst is 43.25 times that of the commercial Pd / C.

[0032] Example 2

[0033] Chloropaldic acid was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of a commercial mixed phase titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0034] Example 3

[0035] Palladium iodide was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial rutile titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0036] Example 4

[0037] Palladium bromide was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial zinc oxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / ZnO single atom catalyst with ZnO as the carrier and containing 0.4 wt% Pd.

[0038] Example 5

[0039] Palladium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial tungsten oxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / WO3 single atom catalyst with WO3 as a carrier and containing 0.4 wt% Pd.

[0040] Example 6

[0041] Chloropaldic acid was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial cerium oxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / CeO2 single atom catalyst with CeO2 as the carrier and containing 0.4 wt% Pd.

[0042] Example 7

[0043] Disperse chloroplatinic acid in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, then add 50 mg of commercial titanium dioxide and irradiate with ultraviolet light in air for 4 hours. After the reaction is completed, filter the obtained product, wash it with deionized water and ethanol respectively, and dry it to obtain a Pt / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pt.

[0044] Example 8

[0045] Rhodium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Rh / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Rh.

[0046] Example 9

[0047] Ruthenium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Ru / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Ru.

[0048] Example 10

[0049] Disperse chloroiridic acid in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, then add 50 mg of commercial titanium dioxide and irradiate with ultraviolet light in air for 4 hours. After the reaction is completed, filter the obtained product, wash it with deionized water and ethanol respectively, and dry it to obtain an Ir / TiO2 single atom catalyst with TiO2 as a carrier and containing 0.5 wt% Ir.

[0050] Embodiment 11

[0051] Disperse ferric chloride in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 1 mol / L, then add 50 mg of commercial titanium dioxide and irradiate with ultraviolet light in air for 4 hours. After the reaction is completed, filter the obtained product, wash it with deionized water and ethanol respectively, and dry it to obtain a Fe / TiO2 single-atom catalyst with TiO2 as a carrier and containing 1 wt% Fe.

[0052] Example 12

[0053] Cobalt chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 2 mol / L, and then 50 mg of commercial titanium dioxide was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Co / TiO2 single-atom catalyst with TiO2 as a carrier and containing 2 wt% Co.

[0054] Embodiment 13

[0055] Nickel chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 3 mol / L, and then 50 mg of commercial titanium dioxide was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Ni / TiO2 single-atom catalyst with TiO2 as a carrier and containing 3 wt% Ni.

[0056] Embodiment 14

[0057] Palladium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.25 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.2 wt% Pd.

[0058] Embodiment 15

[0059] Palladium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.1 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.08 wt% Pd.

[0060] Example 16

[0061] Palladium chloride was dispersed in 20 mL of acetonitrile to obtain a metal precursor solution with a concentration of 0.05 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.04 wt% Pd.

[0062] Embodiment 17

[0063] Palladium chloride was dispersed in 20 mL of acrylonitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0064] Embodiment 18

[0065] Palladium chloride was dispersed in 20 mL of benzyl cyanide to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0066] Embodiment 19

[0067] Palladium chloride was dispersed in 20 mL of nitriloacetic acid to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.3 wt% Pd.

[0068] Embodiment 20

[0069] Palladium chloride was dispersed in 20 mL of malononitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0070] Embodiment 21

[0071] Palladium chloride was dispersed in 20 mL of benzyl nitrile to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0072] Embodiment 22

[0073] Palladium chloride was dispersed in 20 mL of tripolyamine to obtain a metal precursor solution with a concentration of 0.5 mol / L, and then 50 mg of commercial titanium dioxide catalyst was added and irradiated with ultraviolet light in air for 4 hours. After the reaction was completed, the product was filtered, washed with deionized water and ethanol respectively, and dried to obtain a Pd / TiO2 single-atom catalyst with TiO2 as a carrier and containing 0.4 wt% Pd.

[0074] In Examples 2-22, no nanoparticles were formed in the obtained single-atom catalysts, and isolated metal atoms existed.

[0075] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit the present invention. Any changes, substitutions, modifications, and simplifications made by ordinary technicians in this technical field within the essential scope of the present invention are equivalent transformations, do not depart from the purpose of the present invention, and should also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for synthesizing single-atom metal catalysts by photocatalytic coordination anchoring in one step. It is characterized in that The steps include: Adding metal precursor and photocatalyst powder into nitrile compound and stirring thoroughly; Light irradiation anchors the single atoms on the surface of the photocatalyst; After the reaction is finished, the solid product is taken out, washed and dried to obtain a single atom catalyst; The metal contained in the metal precursor includes a noble metal or a common metal; the noble metal includes one or more of ruthenium, rhodium, iridium, gold, silver, platinum or palladium, and the common metal includes one or more of iron, manganese, chromium, zinc, tin, lead, aluminum, copper, nickel or cobalt; the metal precursor is a metal halide; The nitrile compound includes one or more of acrylonitrile, acetonitrile, benzyl cyanide, nitrile acetic acid, malononitrile, nitrile benzyl or trimeramide; The photocatalyst includes organic photocatalyst, inorganic photocatalyst and composite semiconductor photocatalytic material; The dosage ratio of the photocatalyst to the nitrile compound is (0.25-4) mg / mL; the dosage ratio of the metal element to the nitrile compound in the metal precursor is 0.1-1 mol / L; The wavelength of the light irradiation is 150-1500nm, covering deep ultraviolet light, ultraviolet light, visible light and near infrared light; the irradiation time is 4-8h.

2. The method for synthesizing single-atom metal catalysts by photocatalytic coordination anchoring in one step according to claim 1, Features: The organic photocatalyst includes carbon nitride and an organic porphyrin compound; The inorganic photocatalyst includes titanium dioxide, bismuth oxyhalide and cadmium sulfide; The composite semiconductor photocatalytic material comprises porphyrin-sensitized titanium dioxide, carbon nitride-loaded oxyhalogen bismuth, and carbon dot-modified titanium dioxide.

3. The single atom catalyst prepared according to the method according to any one of claims 1 to 2.

4. The single atom catalyst according to claim 3, Features: The loading amount of the metal single atom is 0.01% to 5%.

Citation Information

Patent Citations