A kind of resin infiltrated ceramic and preparation method thereof
By using polymethyl methacrylate modified sodium aluminum silicate and cage silsesquioxane and acrylate resin, the problem of mismatch between the existing resin-permeable ceramic materials and the mechanical properties of the teeth was solved, and the mechanical properties of the existing resin-permeable ceramic materials were prepared. Resin permeable ceramic with excellent mechanical properties and low shrinkage, suitable for dental restoration.
Patent Information
- Application Number
- CN202211687527.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing resin-permeable ceramic materials have a large difference from human teeth in mechanical properties, resulting in mismatch in wear and occlusal stress, making it difficult to use in dental restoration.
Polymethyl methacrylate modified sodium aluminum silicate is used as the ceramic body material, and cage-type silsesquioxane containing methacrylate functional groups is combined with acrylate resin to make it through in-situ polymerization and permeation. The curing method forms a resin-permeable ceramic with excellent mechanical properties.
It achieves fracture toughness, flexural strength and hardness similar to human teeth, and has low shrinkage characteristics. It is suitable as a dental crown bridge restoration material and is easy to cut by CAD/CAM.
Smart Images

Figure BDA0004020041800000041 
Figure BDA0004020041800000051 
Figure BDA0004020041800000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resin-infiltrated ceramics, and in particular to a resin-infiltrated ceramic and a preparation method thereof. Background Art
[0002] Resin-infiltrated ceramics are a new type of composite transparent ceramic material with an interpenetrating network structure formed by infiltrating resin into porous ceramic scaffolds. It is at the forefront of the development of digital crown and bridge restoration diagnosis and treatment as well as innovative material research and development in the oral cavity.
[0003] CN106007802 A discloses a resin-infiltrated ceramic composite material and a preparation method thereof. The resin-infiltrated ceramic selects yttria-stabilized tetragonal zirconium oxide as a porous ceramic body, and the mixed resin is a methacrylate resin and a benzoyl peroxide thermal curing agent. The mechanical properties of the prepared resin-infiltrated ceramic are relatively excellent, but the material is far from human natural teeth, does not have bionic properties and is not suitable for clinical use. For example, the elastic modulus performance of the prepared material is much higher than that of human dentin. When used clinically by patients, the repair material will wear on human natural teeth and cause damage.
[0004] CN107903557 A discloses a dental machinable resin-infiltrated glass-ceramic material and a preparation method thereof. The resin-infiltrated ceramic material selects silanized barium glass-ceramic powder as a porous ceramic blank, and acrylic acid acrylate resin monomer and benzoyl peroxide as the resin to be infiltrated. The dental restoration resin-infiltrated glass-ceramic material having mechanical properties similar to those of human teeth is prepared, but its elastic modulus is lower than that of natural teeth.
[0005] CN108578250 A discloses a resin-infiltrated silicate composite material and a preparation method thereof. The resin is selected from common bisphenol A dimethacrylate glycidyl and triethylene glycol dimethacrylate, and the curing agent is selected from benzoyl peroxide and the like as the resin to be infiltrated. The resin is infiltrated into a porous ceramic block by vacuum capillary action, and then cured to form a silicate / resin double network structure. The bending strength and hardness of the resin-infiltrated silicate composite material are low.
[0006] In the prior art, there is relatively little research on resin-infiltrated ceramics. The ceramic blanks are mostly made of zirconia ceramics, alumina ceramics or glass ceramics to prepare porous ceramic skeletons. The mechanical properties of the resin-infiltrated ceramics formed are significantly different from those of natural teeth. This difference will cause wear to natural teeth or have a negative impact on the transmission of occlusal stress between the restorative materials and natural teeth.
[0007] Therefore, it is necessary to develop a resin-infiltrated ceramic material with an elastic modulus close to that of human teeth. Summary of the invention
[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a resin-infiltrated ceramic and a preparation method thereof. The resin-infiltrated ceramic has excellent mechanical properties, fracture toughness, flexural strength and hardness similar to those of human teeth, and has the characteristics of low shrinkage, is easy to CAD / CAM cutting, and can be used as a dental crown and bridge repair material.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a resin-infiltrated ceramic, the resin-infiltrated ceramic comprising a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0011] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0012] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0013] In the present invention, sodium aluminum silicate modified with polymethyl methacrylate is used as the main material of the ceramic body and is used in combination with a resin system, wherein in the resin system, a cage-type silsesquioxane containing a methacrylate functional group has a structure similar to that of an acrylic resin, thereby achieving a reduction in the polymerization shrinkage of the resin-infiltrated ceramic and ensuring that the introduced material has good compatibility and dispersibility with the acrylic resin; the good interface compatibility between the sodium aluminum silicate modified with polymethyl methacrylate and the acrylic resin can ensure that it has good compatibility and dispersibility with the resin, thereby enabling the resin-infiltrated ceramic to have good fracture toughness, flexural strength and hardness.
[0014] In the present invention, there is no restriction on the acrylic resin monomer for preparing the resin, and it can meet the actual needs. The acrylic monomer can be a monofunctional (meth) acrylate or a multifunctional (meth) acrylate. For example, the acrylic monomer includes but is not limited to methyl (meth) acrylate, ethyl (meth) acrylate, 2-hydroxyethyl (meth) acrylate, butyl (meth) acrylate, benzyl (meth) acrylate, tetrahydrofurfuryl (meth) acrylate or isobornyl (meth) acrylate, methacrylic acid p-cumylphenoxyethylene glycol ester (CMP-1E), methacrylic acid 2-(2-biphenyloxy)ethyl ester, bisphenol A dimethacrylate, bis-GMA (addition product of methacrylic acid and bisphenol A diglycidyl ether), UDMA (methacrylic acid 2-hydroxyethyl and 2,2,4-trimethylolpropane) ester. any one or a mixture of dimethacrylate, dimethacrylate, trimethacrylate, 1,4-butanediol dimethacrylate, 1,10-decanediol dimethacrylate (D3MA), bis(methacryloyloxymethyl)tricyclo-[5.2.1.02,6]decane (DCP), polyethylene glycol dimethacrylate or polypropylene glycol dimethacrylate, polyethylene glycol 200 dimethacrylate, polyethylene glycol 400 dimethacrylate or 1,12-dodecanediol dimethacrylate.
[0015] Preferably, based on the total mass of the resin-infiltrated ceramic being 100%, the mass percentage of the ceramic body is 70%-80%, for example, 72%, 74%, 76%, 78%, etc.
[0016] Preferably, based on the total mass of the resin-infiltrated ceramic being 100%, the mass percentage of the resin is 20%-30%, for example, 22%, 24%, 26%, 28%, etc.
[0017] Preferably, the porosity of the ceramic body is 10%-55%, for example, 20%, 30%, 40%, 50%, etc.
[0018] Preferably, the raw materials for preparing the ceramic green body include sodium aluminum silicate, a solvent, a silane coupling agent, methyl methacrylate monomer and an initiator.
[0019] Preferably, the particle size of the sodium aluminum silicate is 0.4-3.2 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, etc.
[0020] Preferably, the solvent comprises anhydrous ethanol.
[0021] Preferably, the initiator comprises azobisisobutyronitrile.
[0022] Preferably, based on the total mass of the raw materials for preparing the ceramic body being 100%, the raw materials for preparing the ceramic body include the following components in terms of mass percentage:
[0023]
[0024] In the present invention, the mass percentage of the sodium aluminum silicate is 20%-40%, such as 25%, 30%, 35%, etc.
[0025] The mass percentage of the solvent is 30%-60%, for example, 35%, 40%, 45%, 50%, 55% and the like.
[0026] The mass percentage of the silane coupling agent is 10%-25%, for example, 12%, 14%, 16%, 18%, 20%, 22%, 24%, etc.
[0027] The mass percentage of the methyl methacrylate monomer is 15%-25%, for example, 16%, 18%, 20%, 22%, 24%, etc.
[0028] The mass percentage of the initiator is 0.02%-0.1%, such as 0.04%, 0.06%, 0.08%, etc.
[0029] Preferably, the structure of the cage-type silsesquioxane containing methacrylate functional groups is (RSiO 3 / 2 )n;
[0030] Wherein, n is 6, 8, 10, 12 or 14, and at least one of R is selected from methacrylate functional groups.
[0031] Cage silsesquioxane (POSS) is a type of organic-inorganic hybrid monomer with a particle size of about 1.5nm and a molecular formula of (RSiO3 / 2)n, where n is generally 6, 8, or 10. The properties of POSS are between those of silicon dioxide (SiO2) and silicone resin (R2SiO)n, with a polyhedral inorganic framework core of SiO nanostructure surrounded by organic groups. The organic groups of functionalized cage silsesquioxane are reactive and can produce good compatibility or chemical bonds with a variety of polymers to form nanoscale inorganic-organic hybrid composite materials.
[0032] Preferably, the structural formula of the cage-type silsesquioxane (POSS-MA) containing methacrylate functional groups is as shown in Formula I:
[0033]
[0034] Here, R is independently selected from hydrogen, methacrylate functional group or other functional group containing unsaturated bond, and methacrylate functional group is more preferred.
[0035] The present invention preferably uses POSS derivatives in which 8 R groups are methacrylate functional groups, i.e., polyhedral oligomeric silsesquioxane-methacrylate (POSS-MA). POSS-MA is combined with acrylic resin, and both have good compatibility and can simultaneously carry out curing reaction. When added to dental resin materials, its inorganic support structure can maintain its spatial structure during polymerization, thereby effectively reducing the volume shrinkage of the material, effectively avoiding the interface cracks between the resin after impregnation and curing and the ceramic skeleton caused by the polymerization volume shrinkage, and giving the resin infiltration ceramic material excellent mechanical properties.
[0036] All acrylate-based POSSs involved in the present invention can be synthesized by themselves or purchased through commercial channels.
[0037] Preferably, the raw materials for preparing the resin further include a thermal initiator.
[0038] Preferably, the thermal initiator comprises any one of dicumyl peroxide, tert-butyl peroxide or benzoyl peroxide, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of dicumyl peroxide and tert-butyl peroxide, a combination of tert-butyl peroxide and benzoyl peroxide, a combination of dicumyl peroxide, tert-butyl peroxide and benzoyl peroxide, and the like.
[0039] Preferably, the tert-butyl peroxide comprises tert-butyl peroxyacetate and / or tert-butyl perbenzoate.
[0040] Preferably, based on the total mass of the raw materials for preparing the resin being 100%, the raw materials for preparing the resin include the following components in terms of mass percentage:
[0041] Acrylate resin monomer 70%-95%
[0042] Cage-type silsesquioxane containing methacrylate functional groups 0.003%-18%
[0043] Thermal initiator 0.35%-2%.
[0044] In the present invention, the mass percentage of the acrylic resin monomer is 70%-95%, such as 75%, 80%, 85%, etc.
[0045] The mass percentage of the cage-type silsesquioxane containing methacrylate functional groups is 0.003%-18%, for example, 0.5%, 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, etc.
[0046] The mass percentage of the thermal initiator is 0.35%-2%, such as 0.5%, 1%, 1.5%, etc.
[0047] In a second aspect, the present invention provides a method for preparing the resin-infiltrated ceramic according to the first aspect, the preparation method comprising the following steps: infiltrating a resin into a ceramic body to obtain the resin-infiltrated ceramic.
[0048] Preferably, the preparation method comprises the following steps:
[0049] (1) mixing an acrylic resin monomer, a thermal initiator and a cage-type silsesquioxane containing a methacrylate functional group, and reacting the mixture to obtain the resin;
[0050] The sodium aluminum silicate, solvent, silane coupling agent, methyl methacrylate monomer and initiator are mixed, polymerized in situ, and pressed to obtain the ceramic body;
[0051] (2) Immersing the ceramic body in resin, infiltrating and curing, to obtain the resin-infiltrated ceramic.
[0052] Preferably, in step (1), the in-situ polymerization comprises:
[0053] (a) mixing and dispersing sodium aluminum silicate, a solvent, a silane coupling agent and a methyl methacrylate monomer, heating for reaction, and post-processing;
[0054] (b) mixing the post-treated raw materials of step (a), methyl methacrylate monomer and initiator, and reacting them to complete in-situ polymerization.
[0055] In the present invention, sodium aluminum silicate with low cost is selected as the porous ceramic scaffold of resin infiltration ceramics. The main purpose is to graft polymethyl methacrylate (PMMA) to the surface of sodium aluminum silicate by an in-situ polymerization method for interface modification, so as to obtain a PMMA-coated sodium aluminum silicate nanocomposite material as a ceramic skeleton material of resin infiltration ceramics. On the one hand, the uniform dispersibility of sodium aluminum silicate in the resin infiltration ceramics can be improved, and the formation of interpenetrating network channels can be facilitated. On the other hand, the interface compatibility between sodium aluminum silicate and acrylic resin can be improved, because sodium aluminum silicate and PMMA are completely combined by a stable chemical bond, which is equivalent to the PMMA molecular chain "growing" on the sodium aluminum silicate nanoparticles, so there is no difference between the inorganic phase and the organic phase. The mechanical properties of the resin infiltration ceramics prepared in this way are significantly improved, thereby providing a resin infiltration ceramic material with excellent mechanical properties (fracture toughness, flexural strength and hardness similar to those of human teeth) and low shrinkage, which is easy to cut by CAD / CAM and used as a dental crown and bridge repair material.
[0056] Preferably, in step (a), the mixing and dispersing methods include stirring and ultrasound.
[0057] Preferably, the temperature of the heating reaction is 70-90°C, such as 75°C, 80°C, 85°C, etc.
[0058] Preferably, the heating reaction time is 1-5 h, for example, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, etc.
[0059] Preferably, the post-treatment comprises washing and drying.
[0060] Preferably, in step (b), the mixing comprises first mixing the post-treated raw material in step (a) with methyl methacrylate monomer, and then mixing with the initiator.
[0061] Preferably, the reaction includes a first reaction, a second reaction and a third reaction.
[0062] Preferably, the temperature of the first reaction is 70-80° C. (eg, 72° C., 74° C., 76° C., 78° C., etc.) until the system begins to become viscous.
[0063] Preferably, the first reaction time is 3-5 h, such as 3.5 h, 4.5 h, 5 h, etc.
[0064] Preferably, the temperature of the second reaction is 40-60°C, such as 45°C, 50°C, 55°C, etc.
[0065] Preferably, the second reaction time is 10-30 h, such as 15 h, 20 h, 25 h, etc.
[0066] Preferably, the temperature of the third reaction is 90-110°C, such as 95°C, 100°C, 105°C, etc.
[0067] Preferably, the third reaction time is 1-5 h, for example, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, etc.
[0068] Preferably, the pressing pressure is 1-10 MPa, such as 2 MPa, 4 MPa, 6 MPa, 8 MPa, etc.
[0069] Preferably, the pressing time is 1-5 min, such as 2 min, 3 min, 4 min, etc.
[0070] Preferably, in step (2), the infiltration is performed under vacuum.
[0071] Preferably, the penetration time is 3-4 h, such as 3.2 h, 3.4 h, 3.6 h, 3.8 h, etc.
[0072] Preferably, the curing temperature is 120-160°C, such as 130°C, 140°C, 150°C, etc.
[0073] Preferably, the curing pressure is 200-300 MPa, such as 220 MPa, 240 MPa, 260 MPa, 280 MPa, etc.
[0074] Preferably, the curing time is 60-90 min, for example, 65 min, 70 min, 75 min, 80 min, 85 min, etc.
[0075] As a preferred technical solution, the preparation method comprises the following steps:
[0076] (1) mixing an acrylic resin monomer, a thermal initiator and a cage-type silsesquioxane containing a methacrylate functional group, and reacting the mixture to obtain the resin;
[0077] Sodium aluminum silicate, solvent, silane coupling agent and methyl methacrylate monomer are mixed and dispersed under stirring and ultrasound, and then reacted at 70-90° C. for 1-5 hours, and then washed and dried, and the obtained raw material is sequentially mixed with methyl methacrylate monomer and initiator, and then reacted at 70-80° C. until the system begins to be viscous, and then reacted at 40-60° C. for 10-30 hours, and finally reacted at 90-110° C. for 1-5 hours to obtain a ceramic body raw material;
[0078] The ceramic body raw material is soaked in the dispersion liquid, and pressed at 1-10 MPa for 1-5 minutes to obtain the ceramic body;
[0079] (2) Immersing the ceramic body in resin, infiltrating for 3-4 hours under vacuum, and curing for 60-90 minutes at a temperature of 120-160° C. and a pressure of 200-300 MPa to obtain the resin-infiltrated ceramic.
[0080] Compared with the prior art, the present invention has the following beneficial effects:
[0081] (1) The resin-infiltrated ceramics of the present invention have excellent mechanical properties, with fracture toughness, flexural strength and hardness close to those of human teeth, and have low shrinkage characteristics, are easy to CAD / CAM cut, and can be used as dental crown and bridge repair materials.
[0082] (2) The elastic modulus of the resin-infiltrated ceramics of the present invention is between 20.5±1.4-24.2±1.4 GPa, the bending strength is between 211.8±5.4-291.8±8.1 MPa, the Vickers hardness is between 2.2±0.2-3.3±0.2 GPa, and the shrinkage is within 1.87%. DETAILED DESCRIPTION
[0083] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0084] Example 1
[0085] This embodiment provides a resin-infiltrated ceramic, which includes a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0086] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0087] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0088] In this embodiment, the structural formula of the cage-type silsesquioxane (POSS-MA) containing methacrylate functional groups is shown in Formula I:
[0089]
[0090] Wherein, R is a methacrylate functional group.
[0091] The resin-infiltrated ceramic is obtained by the following preparation method, which comprises the following steps:
[0092] (1) Preparation of resin
[0093] 0.5% benzoyl peroxide and 5% POSS-MA were introduced into triethylene glycol dimethacrylate, and stirred at 150 rev / min at room temperature for 1 h. Then, bisphenol A glycidyl methacrylate was weighed in a ratio of 5:5 and placed in the above system. The mixture was stirred for 2 h until fully mixed and then taken out for use.
[0094] (2) Preparation of Sodium Aluminum Silicate Ceramic Powder
[0095] Take 1000mL of anhydrous ethanol, 30g of KH-570 and 30g of sodium aluminum silicate powder and add them to a 3000mL three-necked flask, stir and disperse them in an ultrasonic cleaner for 15 minutes, and then heat and reflux them in an 80℃ water bath for 3 hours. After the reaction is completed, centrifuge and wash the precipitate with anhydrous ethanol and distilled water for 3 times respectively, vacuum dry, and finally grind it with a mortar to obtain the modified sodium aluminum silicate for use.
[0096] Add 300mL MMA to a 3000mL three-necked flask, then add 600g modified sodium aluminum silicate, add AIBN after ultrasonic oscillation dispersion for 30min, and stir in a 75℃ water bath for prepolymerization. When the system starts to become viscous after 3 hours of reaction, quickly pour it into a 50mL test tube, continue polymerization in a 50℃ water bath for 20h, and finally raise the temperature to 100℃ and react for 3h. Cool and demold to obtain polymethyl methacrylate modified sodium aluminum silicate, which is sodium aluminum silicate ceramic powder.
[0097] (3) Preparation of ceramic green body
[0098] Weigh 100 g of the sodium aluminum silicate ceramic powder prepared above, add 20 mL of 3% polyvinyl alcohol aqueous solution to evenly soak it, place it in an oven at 80°C to dry, then transfer the powder to a steel mold, apply a pressure of 5 MPa, and press for 3 minutes to form a ceramic body with a porosity of 25%.
[0099] (4) Preparation of resin-infiltrated ceramics
[0100] The ceramic body prepared in the above steps is completely immersed in the resin system and placed in a vacuum device as a whole to ensure that the vacuum degree is -0.1 MPa. The vacuum state is maintained for 3 hours to ensure that the body is completely infiltrated by the resin system.
[0101] The sodium aluminum silicate ceramic body completely impregnated with resin is placed in a constant temperature isostatic press and cured at 130° C. and 300 MPa for 60 minutes under high temperature and high pressure to obtain a translucent sodium aluminum silicate-based resin-infiltrated ceramic block, namely the resin-infiltrated ceramic.
[0102] Example 2
[0103] This embodiment provides a resin-infiltrated ceramic, which includes a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0104] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0105] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0106] The difference between the preparation method of this embodiment and that of embodiment 1 lies in the preparation of sodium aluminum silicate ceramic powder in step (2), and the rest is the same as that in embodiment 1. Step (2) of this embodiment is specifically as follows:
[0107] Take 1000mL of anhydrous ethanol, 30g of KH-570 and 30g of sodium aluminum silicate powder and add them to a 3000mL three-necked flask, stir and disperse them in an ultrasonic cleaner for 15 minutes, and then heat and reflux them in an 80℃ water bath for 3 hours. After the reaction is completed, centrifuge and wash the precipitate with anhydrous ethanol and distilled water for 3 times respectively, vacuum dry, and finally grind it with a mortar to obtain the modified sodium aluminum silicate for use.
[0108] Add 300mL MMA to a 3000mL three-necked flask, then add 300g of modified sodium aluminum silicate, add AIBN after ultrasonic oscillation dispersion for 30min, and stir in a 75℃ water bath for prepolymerization. Observe the reactant, and when it begins to become viscous, quickly pour it into a 50mL test tube, continue polymerization in a 50℃ water bath for 20h, and finally raise the temperature to 100℃ and react for 3h. Cool and demold to obtain polymethyl methacrylate modified sodium aluminum silicate, which is sodium aluminum silicate ceramic powder.
[0109] Example 3
[0110] This embodiment provides a resin-infiltrated ceramic, which includes a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0111] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0112] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0113] The difference between the preparation method of this embodiment and that of embodiment 1 lies in the preparation of sodium aluminum silicate ceramic powder in step (2), and the rest is the same as that in embodiment 1. Step (2) of this embodiment is specifically as follows:
[0114] Take 1000mL of anhydrous ethanol, 30g of KH-570 and 30g of sodium aluminum silicate powder and add them to a 3000mL three-necked flask. Stir and disperse them in an ultrasonic cleaner for 15 minutes, then heat and reflux them in a water bath at 80℃ for 3 hours. After the reaction is completed, centrifuge and wash the precipitate with anhydrous ethanol and distilled water for 3 times respectively, vacuum dry, and finally grind it in a mortar for later use.
[0115] Add 300mL MMA to a 3000mL three-necked flask, then add 100g modified sodium aluminum silicate, add AIBN after ultrasonic oscillation dispersion for 30min, and stir in a 75℃ water bath for prepolymerization. Observe the reactant, and when it begins to become viscous, quickly pour it into a 50mL test tube, continue polymerization in a 50℃ water bath for 20h, and finally raise the temperature to 100℃ and react for 3h. Cool and demold to obtain polymethyl methacrylate modified sodium aluminum silicate, which is sodium aluminum silicate ceramic powder.
[0116] Example 4
[0117] This embodiment provides a resin-infiltrated ceramic, which includes a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0118] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0119] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0120] In this embodiment, the cage-type silsesquioxane containing methacrylate functional groups is the same as that in Embodiment 1.
[0121] The resin-infiltrated ceramic is obtained by the following preparation method, which comprises the following steps:
[0122] (1) Preparation of resin
[0123] 1.5% benzoyl peroxide and 12% POSS-MA were introduced into triethylene glycol dimethacrylate, and stirred at 150 rev / min at room temperature for 1 h. Then, UDMA (addition product of 2-hydroxyethyl methacrylate and 2,2,4-trimethylhexamethylene-1,6-diisocyanate) was weighed in a ratio of 3:7 and placed in the above system. The mixture was stirred for 2 h until fully mixed and taken out for use.
[0124] (2) Preparation of Sodium Aluminum Silicate Ceramic Powder
[0125] Take 1000mL of anhydrous ethanol, 30g of KH-570 and 120g of sodium aluminum silicate powder and add them to a 3000mL three-necked flask, stir and disperse them in an ultrasonic cleaner for 20 minutes, and then heat and reflux them in an 80℃ water bath for 3 hours. After the reaction is completed, centrifuge and wash the precipitate with anhydrous ethanol and distilled water for 3 times respectively, vacuum dry, and finally grind it with a mortar to obtain the modified sodium aluminum silicate for use.
[0126] Add 400mL MMA to a 3000mL three-necked flask, then add 80g of modified sodium aluminum silicate, add AIBN after ultrasonic oscillation dispersion for 30min, and stir in a 72℃ water bath for prepolymerization. After 5 hours of reaction, the system begins to become viscous. At this time, pour it into a 1000mL beaker and continue to polymerize in a 60℃ water bath for 15h. Finally, raise the temperature to 105℃ and react for 4h. Cool and demold to obtain polymethyl methacrylate modified sodium aluminum silicate, which is sodium aluminum silicate ceramic powder.
[0127] (3) Preparation of ceramic green body
[0128] Weigh 100 g of the sodium aluminum silicate ceramic powder prepared above, add 20 mL of 3% polyvinyl alcohol aqueous solution to evenly wet it, place it in an oven at 80°C to dry, then transfer the powder to a steel mold, apply a pressure of 6 MPa, and press for 2 minutes to form a ceramic body with a porosity of 22%.
[0129] (4) Preparation of resin-infiltrated ceramics
[0130] The ceramic body prepared in the above steps is completely immersed in the resin system and placed in a vacuum device as a whole to ensure that the vacuum degree is -0.1 MPa. The vacuum state is maintained for 3.5 hours to ensure that the body is completely infiltrated by the resin system.
[0131] The sodium aluminum silicate ceramic body completely impregnated with resin is placed in a constant temperature isostatic press and cured at 140°C and 250MPa for 70 minutes under high temperature and high pressure to obtain a translucent sodium aluminum silicate-based resin-infiltrated ceramic block, namely the resin-infiltrated ceramic.
[0132] Example 5
[0133] This embodiment provides a resin-infiltrated ceramic, which includes a ceramic body and a resin disposed inside and on the surface of the ceramic body;
[0134] The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate;
[0135] The raw materials for preparing the resin include acrylic resin monomers and cage-type silsesquioxane containing methacrylate functional groups.
[0136] In this embodiment, the cage-type silsesquioxane containing methacrylate functional groups is the same as that in Embodiment 1.
[0137] The resin-infiltrated ceramic is obtained by the following preparation method, which comprises the following steps:
[0138] (1) Preparation of resin
[0139] 1.5% benzoyl peroxide and 8% POSS-MA were introduced into 1,10-decanediol dimethacrylate, and stirred at 150 rev / min at room temperature for 1 hour. Then, bisphenol A glycidyl methacrylate was weighed in a ratio of 4:6 and placed in the above system. The mixture was stirred for 2 hours until fully mixed and then taken out for use.
[0140] (2) Preparation of Sodium Aluminum Silicate Ceramic Powder
[0141] Take 1000mL of anhydrous ethanol, 30g of KH-570 and 120g of sodium aluminum silicate powder and add them to a 3000mL three-necked flask, stir and disperse them in an ultrasonic cleaner for 20 minutes, and then heat and reflux them in an 80℃ water bath for 3 hours. After the reaction is completed, centrifuge and wash the precipitate with anhydrous ethanol and distilled water for 3 times respectively, vacuum dry, and finally grind it with a mortar to obtain the modified sodium aluminum silicate for use.
[0142] Add 400mL MMA to a 3000mL three-necked flask, then add 80g of modified sodium aluminum silicate, add AIBN after ultrasonic oscillation dispersion for 30min, and stir in a 78℃ water bath for prepolymerization. After 3.5 hours of reaction, the system begins to become viscous. At this time, quickly pour it into a 1000mL beaker and continue to polymerize in a 60℃ water bath for 15h. Finally, raise the temperature to 110℃ and react for 3h. Cool and demold to obtain polymethyl methacrylate modified sodium aluminum silicate, which is sodium aluminum silicate ceramic powder.
[0143] (3) Preparation of ceramic green body
[0144] Weigh 100 g of the sodium aluminum silicate ceramic powder prepared above, add 25 mL of 3% polyvinyl alcohol aqueous solution to evenly wet it, place it in an oven at 80°C to dry, then transfer the powder to a steel mold, apply a pressure of 6 MPa, and press for 2 minutes to form a ceramic body with a porosity of 28%.
[0145] (4) Preparation of resin-infiltrated ceramics
[0146] The ceramic body prepared in the above steps is completely immersed in the resin system and placed in a vacuum device as a whole to ensure that the vacuum degree is -0.1 MPa. The vacuum state is maintained for 4 hours to ensure that the body is completely infiltrated by the resin system.
[0147] The sodium aluminum silicate ceramic body completely impregnated with resin is placed in a constant temperature isostatic press and cured at 140° C. and 220 MPa for 90 minutes under high temperature and high pressure to obtain a translucent sodium aluminum silicate-based resin-infiltrated ceramic block, namely the resin-infiltrated ceramic.
[0148] Example 6
[0149] The difference between this embodiment and embodiment 1 is that in the cage-type silsesquioxane containing methacrylate functional groups, R is vinyl, and the rest is the same as embodiment 1.
[0150] Comparative Example 1
[0151] The difference between this comparative example and Example 1 is that the ceramic body is unmodified sodium aluminum silicate, that is, step (2) is not included in the preparation, sodium aluminum silicate is used in step (3), and the rest is the same as Example 1.
[0152] Comparative Example 2
[0153] The difference between this comparative example and Example 1 is that in the raw material for preparing the resin, the cage-type silsesquioxane containing methacrylate functional groups is replaced by a cage-type silsesquioxane not containing methacrylate functional groups, the structural formula of which is as follows, R is vinyl, and the rest is the same as Example 1.
[0154]
[0155] Comparative Example 3
[0156] The difference between this comparative example and Example 1 is that in the raw material for preparing the resin, the cage-type silsesquioxane containing methacrylate functional groups is replaced by a cage-type silsesquioxane not containing methacrylate functional groups, the structural formula of which is as follows, R is an aldehyde group, and the rest is the same as Example 1.
[0157]
[0158] Comparative Example 4
[0159] The difference between this comparative example and Example 1 is that the sodium aluminum silicate is replaced with an equal mass of zirconium oxide, and the rest is the same as Example 1.
[0160] Performance Testing
[0161] The resin-infiltrated ceramics described in Examples 1-6 and Comparative Examples 1-4 and human teeth as blank comparative examples were tested as follows:
[0162] (1) Elastic modulus and flexural strength: The resin-infiltrated ceramic was cut into test pieces of 1.2 mm × 4.0 mm × 18 mm. The surface was then polished using 2000-grit sandpaper. A three-point bending test was performed using a tensile testing machine at a fulcrum spacing of 12 mm and a crosshead speed of 1.0 mm / min. The average value of ten specimens was used for evaluation.
[0163] (2) Vickers hardness: Use 2000 grit sandpaper to polish the test surface of the resin-infiltrated ceramic to ensure that the surface of the sample is smooth. Use a Vickers hardness tester to test: select "2" for the test force value; measure 3 different positions of the resin-infiltrated ceramic and calculate the average value.
[0164] (3) Shrinkage: The shrinkage of resin-infiltrated ceramics is characterized by volume shrinkage, that is, the volume shrinkage is calculated by measuring the density of the same resin-infiltrated ceramic block before and after curing.
[0165]
[0166] The test results are summarized in Table 1.
[0167] Table 1
[0168]
[0169] Analysis of the data in Table 1 shows that the elastic modulus of the resin-infiltrated ceramic of the present invention is between 20.5±1.4-24.2±1.4 GPa, the flexural strength is between 211.8±5.4-291.8±8.1 MPa, the Vickers hardness is between 2.2±0.2-3.3±0.2 GPa, and the shrinkage rate is within 1.87%; the resin-infiltrated ceramic of the present invention has excellent mechanical properties, and has fracture toughness, flexural strength and hardness similar to those of human teeth, and has the characteristics of low shrinkage, is easy to CAD / CAM cutting, and can be used as a dental crown and bridge repair material.
[0170] Analysis of comparative examples 1-4 and example 1 shows that the performance of comparative examples 1-4 is not as good as that of example 1, which proves that the resin infiltrated ceramics of the present invention have better performance.
[0171] Analysis of Example 6 and Example 1 shows that the performance of Example 6 is not as good as that of Example 1, which proves that the R groups in the cage-type silsesquioxane containing methacrylate functional groups are preferably methacrylate functional groups, which is more conducive to improving the performance of resin-infiltrated ceramics.
[0172] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A resin-infiltrated ceramic, characterized in that: The resin-infiltrated ceramic comprises a ceramic body and a resin disposed inside and on the surface of the ceramic body; The ceramic body comprises sodium aluminum silicate modified by polymethyl methacrylate; Taking the total mass of the raw materials for preparing the resin as 100%, the raw materials for preparing the resin are composed of the following components in terms of mass percentage: Acrylate resin monomer 70%-95% Cage-type silsesquioxane containing methacrylate functional groups 0.003%-18% Thermal initiator 0.35%-2%; The structural formula of the cage-type silsesquioxane containing methacrylate functional groups is shown in Formula I: Wherein, R is selected from methacrylate functional groups.
2. The resin-infiltrated ceramic according to claim 1, characterized in that: Taking the total mass of the resin-infiltrated ceramic as 100%, the mass percentage of the ceramic body is 70%-80%.
3. The resin-infiltrated ceramic according to claim 1, characterized in that: Taking the total mass of the resin-infiltrated ceramic as 100%, the mass percentage of the resin is 20%-30%.
4. The resin-infiltrated ceramic according to claim 1, characterized in that: The porosity of the ceramic body is 10%-55%.
5. The resin-infiltrated ceramic according to claim 1, characterized in that: The raw materials for preparing the ceramic green body include sodium aluminum silicate, a solvent, a silane coupling agent, a methyl methacrylate monomer and an initiator.
6. The resin-infiltrated ceramic according to claim 5, characterized in that: The particle size of the sodium aluminum silicate is 0.4-3.2 μm.
7. The resin-infiltrated ceramic according to claim 5, characterized in that: The solvent includes anhydrous ethanol.
8. The resin-infiltrated ceramic according to claim 5, characterized in that: The initiator includes azobisisobutyronitrile.
9. The resin-infiltrated ceramic according to claim 5, characterized in that: Taking the total mass of the raw materials for preparing the ceramic body as 100%, the raw materials for preparing the ceramic body include the following components in terms of mass percentage:
10. The resin-infiltrated ceramic according to claim 1, characterized in that The thermal initiator includes any one of dicumyl peroxide, tert-butyl peroxide or benzoyl peroxide, or a combination of at least two thereof.
11. The resin-infiltrated ceramic according to claim 10, characterized in that: The tert-butyl peroxide includes tert-butyl peroxyacetate and / or tert-butyl perbenzoate.
12. A method for preparing the resin-infiltrated ceramic according to any one of claims 1 to 11, characterized in that: The preparation method comprises the following steps: infiltrating resin into a ceramic body to obtain the resin-infiltrated ceramic.
13. The preparation method according to claim 12, characterized in that: The preparation method comprises the following steps: (1) mixing an acrylic resin monomer, a thermal initiator and a cage-type silsesquioxane containing a methacrylate functional group, and reacting the mixture to obtain the resin; The sodium aluminum silicate, solvent, silane coupling agent, methyl methacrylate monomer and initiator are mixed, polymerized in situ, and pressed to obtain the ceramic body; (2) Immersing the ceramic body in resin, infiltrating and curing, to obtain the resin-infiltrated ceramic.
14. The preparation method according to claim 13, characterized in that: In step (1), the in-situ polymerization comprises: (a) mixing and dispersing sodium aluminum silicate, a solvent, a silane coupling agent and a methyl methacrylate monomer, heating for reaction, and post-processing; (b) mixing the post-treated raw materials of step (a), methyl methacrylate monomer and initiator, and reacting them to complete in-situ polymerization.
15. The preparation method according to claim 14, characterized in that: In step (a), the mixing and dispersing methods include stirring and ultrasound.
16. The preparation method according to claim 14, characterized in that: The temperature of the heating reaction is 70-90°C.
17. The preparation method according to claim 14, characterized in that: The heating reaction time is 1-5h.
18. The preparation method according to claim 14, characterized in that: The post-treatment includes washing and drying.
19. The preparation method according to claim 14, characterized in that: In step (b), the mixing includes first mixing the raw material after the treatment in step (a) with methyl methacrylate monomer, and then mixing with the initiator.
20. The preparation method according to claim 14, characterized in that: The reaction includes a first reaction, a second reaction and a third reaction.
21. The preparation method according to claim 20, characterized in that: The temperature of the first reaction is 70-80° C., until the system begins to become viscous.
22. The preparation method according to claim 20, characterized in that: The time of the first reaction is 3-5h.
23. The preparation method according to claim 20, characterized in that: The temperature of the second reaction is 40-60°C.
24. The preparation method according to claim 20, characterized in that: The second reaction time is 10-30h.
25. The preparation method according to claim 20, characterized in that: The temperature of the third reaction is 90-110°C.
26. The preparation method according to claim 20, characterized in that: The time of the third reaction is 1-5h.
27. The resin-infiltrated ceramic according to claim 13, characterized in that The pressing pressure is 1-10 MPa.
28. The preparation method according to claim 13, characterized in that: The pressing time is 1-5 min.
29. The preparation method according to claim 13, characterized in that: In step (2), the infiltration is performed under vacuum.
30. The preparation method according to claim 13, characterized in that: The penetration time is 3-4h.
31. The preparation method according to claim 13, characterized in that: The curing temperature is 120-160°C.
32. The preparation method according to claim 13, characterized in that: The curing pressure is 200-300 MPa.
33. The preparation method according to claim 13, characterized in that: The curing time is 60-90 minutes.
34. The preparation method according to claim 13, characterized in that: The preparation method comprises the following steps: (1) mixing an acrylic resin monomer, a thermal initiator and a cage-type silsesquioxane containing a methacrylate functional group, and reacting the mixture to obtain the resin; Sodium aluminum silicate, solvent, silane coupling agent and methyl methacrylate monomer are mixed and dispersed under stirring and ultrasound, and then reacted at 70-90° C. for 1-5 hours, and then washed and dried, and the obtained raw material is sequentially mixed with methyl methacrylate monomer and initiator, and then reacted at 70-80° C. until the system begins to be viscous, and then reacted at 40-60° C. for 10-30 hours, and finally reacted at 90-110° C. for 1-5 hours to obtain a ceramic body raw material; The ceramic body raw material is soaked in the dispersion liquid, and pressed at 1-10 MPa for 1-5 minutes to obtain the ceramic body; (2) Immersing the ceramic body in resin, infiltrating for 3-4 hours under vacuum, and curing for 60-90 minutes at a temperature of 120-160° C. and a pressure of 200-300 MPa to obtain the resin-infiltrated ceramic.