Polyethylene for artificial grass and special material for artificial grass and preparation method and application thereof

By using Ziegler-Natta catalyst to synthesize polyethylene in the production of artificial turf fibers, and combining antioxidants and extrusion preparation methods, the phase separation problem of polyethylene artificial turf special materials and the high cost of catalysts in the existing technology are solved. problem, achieving high-performance and low-cost production of polyethylene artificial grass.

CN116023571BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111243280.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-10-15
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

The existing artificial turf fiber production is not standardized and the research and development of high-performance monofilament turf yarn is insufficient, which leads to the problems of serious phase separation, uneven mixing and high catalyst cost in the production of polyethylene artificial turf special materials.

Method used

Polyethylene is synthesized in a slurry polymerization reaction using a Ziegler-Natta catalyst (TiCl4/MgCl2), and an alkyl aluminum cocatalyst and hydrogen are added as a molecular weight regulator, together with hindered phenols and phosphite antioxidants. Special materials for artificial grass are produced by slurry polymerization and extrusion preparation methods.

Benefits of technology

It improves the processing performance and mechanical properties of polyethylene artificial grass, reduces catalyst costs, meets production requirements, reduces downstream production costs and energy consumption, and improves product quality and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a polyethylene for artificial grass and a special material for artificial grass, and a preparation method and application thereof. A polyethylene for artificial grass is obtained by slurry polymerization of ethylene and α-olefin in the presence of a Ziegler-Natta catalyst. The special material for artificial grass prepared by using the polyethylene has good processing performance and excellent mechanical properties, can meet the production requirements of polyethylene artificial grass manufacturers, and has low production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to polyethylene for artificial grass and special material for artificial grass, as well as preparation methods and applications thereof. Background Art

[0002] Although there are hundreds of companies engaged in artificial turf production in China, the fiber production of artificial turf is not standardized, and the research and development of high-performance monofilament turf yarn is almost blank. Most of them are low-grade products with extensive management or products produced by "processing with supplied materials". At present, there is no self-produced polyethylene artificial turf material in China. Artificial turf manufacturers usually use blended materials for drawing (DFDA7042+HDPE+mLLDPE2047, mainly DFDA7042). The melting process is prone to serious phase separation and uneven mixing, which makes the grass yarn easy to age.

[0003] CN103221588B discloses an artificial grass, in particular, an artificial grass formed by cutting a film or a monofilament cluster prepared by using polyethylene, wherein the polyethylene is prepared by using a bis-tetrahydroindenyl or bis-indenyl metallocene catalyst complex, and has (a) a carbon content of 0.910-0.937 g / cm 3 The polyethylene comprises a polyethylene having a density in the range of 0.5 to 5 g / 10 min, the density being determined by ISO 1183 at a temperature of 23° C., and (b) a melt index MI2 in the range of 0.5 to 5 g / 10 min, the melt index MI2 being determined by ISO 1133 / D at a temperature of 190° C. and under a load of 2.16 kg, wherein the polyethylene has a grcio of less than 0.9 or a LCBI of greater than 0.08, and wherein the polyethylene has a Vicat softening temperature Tv measured according to ISO 306 Condition A120 that conforms to the following equation: Tv>41234d2+77500d-36295, wherein Tv is the Vicat softening temperature, expressed in ° C., and d is the density of the polyethylene, expressed in g / cm 3 The artificial grass is prepared by using a di-tetrahydroindenyl or di-indenyl metallocene catalyst complex, which has the problems of expensive catalysts and high costs. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention provides a new polyethylene for artificial turf. The special material for artificial turf prepared by using the polyethylene has good processing performance and excellent mechanical properties, can meet the production requirements of polyethylene artificial turf manufacturers, and the catalyst price is low and the production cost is low.

[0005] In a first aspect, the present invention provides a polyethylene for artificial turf, which is obtained by slurry polymerization of ethylene and α-olefin in the presence of a Ziegler-Natta catalyst.

[0006] According to some embodiments of the polyethylene of the present invention, the catalyst is TiCl4 / MgCl2. In some specific embodiments of the present invention, the catalyst (TiCl4 / MgCl2) used in the reaction can be a commercially available SLC-S, such as but not limited to that purchased from Shanghai Lide Company.

[0007] According to some embodiments of the polyethylene of the present invention, the activity of the catalyst is 17000-38000 kg / kg.

[0008] According to some embodiments of the polyethylene of the present invention, the catalyst further comprises an alkyl aluminum co-catalyst. In the present invention, the alkyl aluminum co-catalyst may be at least one of triethyl aluminum, triethylbutyl aluminum and tri-tert-butyl aluminum.

[0009] According to some embodiments of the polyethylene of the present invention, the reaction further comprises using H2 as a molecular weight regulator.

[0010] According to some embodiments of the polyethylene of the present invention, the α-olefin is selected from at least one of 1-butene, 1-hexene and 1-octene.

[0011] According to some embodiments of the polyethylene of the present invention, the polyethylene for artificial grass has a melt index of 1-5 g / 10 min at 2.16 kg and 190° C., preferably 1-4 g / 10 min.

[0012] According to some embodiments of the polyethylene of the present invention, the molecular weight distribution of the polyethylene for artificial grass is 3-6, preferably 3.8-4.5.

[0013] According to some embodiments of the polyethylene of the present invention, the density of the polyethylene for artificial grass is 0.918-0.940 g / cm 3 , preferably 0.918-0.930 g / cm 3 .

[0014] The second aspect of the present invention provides a method for preparing polyethylene for artificial turf, comprising subjecting ethylene and α-olefin to a slurry polymerization reaction in the presence of a Ziegler-Natta catalyst.

[0015] According to some embodiments of the preparation method of the present invention, the molar ratio of α-olefin to ethylene is 0.24-0.28:1.

[0016] According to some embodiments of the preparation method of the present invention, the method further comprises using H2, preferably, the molar ratio of H2 to ethylene is 0.17-0.23: 1. H2 is used as a molecular weight regulator.

[0017] According to some embodiments of the preparation method of the present invention, the reaction conditions include: a temperature of 85-90° C. and a pressure of 1800-2800 kPa.

[0018] A third aspect of the present invention provides a special material for artificial grass, comprising polyethylene for artificial grass and a compound additive, wherein the polyethylene for artificial grass is the above-mentioned polyethylene for artificial grass or the polyethylene for artificial grass prepared by the above-mentioned method.

[0019] According to some embodiments of the artificial turf material of the present invention, the compound additive includes a hindered phenol antioxidant and a phosphite antioxidant, and more preferably includes antioxidant 1010 and antioxidant 168. The compound additive can be a compound additive with a brand name of CD-9 purchased from Kodak.

[0020] According to some embodiments of the special material for artificial turf of the present invention, based on the total weight of the special material for artificial turf, the content of polyethylene for artificial turf is 99.96-99.98 weight %, and the content of the compound additive is 0.02-0.04 weight %.

[0021] A fourth aspect of the present invention provides a method for preparing a special material for artificial grass, comprising mixing and extruding polyethylene for artificial grass and a compound additive, wherein the polyethylene for artificial grass is the above-mentioned polyethylene for artificial grass or the polyethylene for artificial grass prepared by the above-mentioned method.

[0022] According to some embodiments of the preparation method of the present invention, the mixing conditions include: a temperature of 200-210° C. and a time of 2-4 minutes.

[0023] According to some embodiments of the preparation method of the present invention, the compound additive includes a hindered phenol antioxidant and a phosphite antioxidant, and more preferably includes antioxidant 1010 and antioxidant 168. The compound additive can be a compound additive with a brand name of CD-9 purchased from Kodak.

[0024] According to some embodiments of the preparation method of the present invention, based on the total weight of the special material for artificial turf, the content of polyethylene for artificial turf is 99.96-99.98 wt %, and the content of the compound additive is 0.02-0.04 wt %.

[0025] The fifth aspect of the present invention provides the above polyethylene for artificial grass, the preparation method of the above polyethylene for artificial grass, the above special material for artificial grass or the use of the preparation method of the above special material for artificial grass in artificial turf.

[0026] Beneficial effects of the present invention:

[0027] (1) The artificial turf special material prepared by using the polyethylene for artificial turf of the present invention has good processing performance and excellent mechanical properties, and the grass yarn produced has good flexibility and good wear resistance. The melt index at 2.16kg and 190°C can reach more than 2.45g / 10min, the yield stress can reach more than 12.5MPa, and the yield strain rate can reach more than 17%.

[0028] (2) The polyethylene for artificial turf of the present invention significantly improves the processing performance and mechanical properties of the special material for artificial turf, thereby meeting the production requirements of polyethylene artificial turf manufacturers.

[0029] (3) The artificial grass special material of the present invention can reduce the production cost of downstream processing enterprises, reduce process energy consumption, and improve product quality.

[0030] (4) According to the current price of the blended materials used in downstream, the artificial grass special material of the present invention can generate revenue of 500 yuan / ton, which has good economic and social benefits. DETAILED DESCRIPTION

[0031] In order to make the present invention more easily understood, the present invention will be described in detail below in conjunction with embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.

[0032] The test method of the present invention and the equipment used in the test are as follows:

[0033] (1) The method for determining the melt index at 190°C shall refer to GB / T 3682-2000.

[0034] (2) The density determination method refers to GB / T 1033.2-2010.

[0035] (3) The molecular weight and molecular weight distribution were determined using a high temperature gel permeation chromatograph (purchased from Agilent, model PL-GPC220).

[0036] (4) The determination method of yield stress and yield strain shall refer to GB / T 1040.3-2006.

[0037] The raw materials used in the following examples and comparative examples are as follows:

[0038] (1) SLC-S catalyst was purchased from Shanghai Lide Company.

[0039] (2) CD-9 compound additive was purchased from Kodak.

[0040] (3) The parameters of ethylene are as follows:

[0041]

[0042]

[0043] (4) The parameters of 1-butene are as follows:

[0044] project purity% <![CDATA[H2O content]]> CO content <![CDATA[CO2 content]]> <![CDATA[O2 content]]> <![CDATA[CH3OH content]]> index ≥99.0 <![CDATA[≤100×10 -6 ]]> <![CDATA[≤5×10 -6 ]]> <![CDATA[≤10×10 -6 ]]> <![CDATA[≤1×10 -6 ]]> <![CDATA[≤10×10 -6 ]]>

[0045] (5) The parameters of hydrogen are as follows:

[0046] project purity% <![CDATA[H2O content]]> <![CDATA[CO + CO2 content]]> <![CDATA[O2 content]]> index ≥93.0% <![CDATA[≤5×10 -6 ]]> <![CDATA[≤5×10 -6 ]]> <![CDATA[≤10×10 -6 ]]>

[0047] (6) Triethylaluminum was purchased from Sigma-Aldrich Company with CAS number 97-93-8.

[0048] [Example 1]

[0049] In the presence of a feed rate of 1.6 kg / h of SLC-S catalyst and 300 ppm of triethylaluminum (co-catalyst), ethylene and 1-butene were subjected to a slurry polymerization reaction, and hydrogen as a molecular weight regulator was added simultaneously, wherein the hydrogen / ethylene molar ratio was 0.2, the 1-butene / ethylene molar ratio was 0.23, the reactor pressure was 2300 kPa, the reaction temperature was controlled at 86.5°C, the ethylene partial pressure was 500 kPa, and polyethylene for artificial turf was obtained. The properties of the polyethylene for artificial turf were measured, and the results are shown in Table 1.

[0050] [Example 2]

[0051] The method of Example 1 was followed, except that the 1-butene / ethylene molar ratio was 0.28, and polyethylene for artificial turf was finally obtained.

[0052] [Example 3]

[0053] The method of Example 1 was followed, except that the hydrogen / ethylene molar ratio was 0.17, and polyethylene for artificial turf was finally obtained.

[0054] [Example 4]

[0055] The method of Example 1 was followed, except that the hydrogen / ethylene molar ratio was 0.23, and polyethylene for artificial turf was finally obtained.

[0056] Table 1

[0057]

[0058] [Example 5]

[0059] 99.97 wt % of the polyethylene for artificial turf prepared in Example 1 and 0.03 wt % of CD-9 (compound additive) were mixed in a high-speed mixer at room temperature and pressure for 3 minutes, and then the temperature was controlled at 210° C. and granulated using a twin-screw extruder to obtain a special material for artificial turf. The physical properties of the special material for artificial turf were tested and analyzed, and the results are shown in Table 2.

[0060] [Example 6]

[0061] 99.98 wt % of the polyethylene for artificial turf prepared in Example 1 and 0.02 wt % of CD-9 (compound additive) were mixed in a high-speed mixer at room temperature and pressure for 3 minutes, and then the temperature was controlled at 210° C. and granulated using a twin-screw extruder to obtain a special material for artificial turf. The physical properties of the special material for artificial turf were tested and analyzed, and the results are shown in Table 2.

[0062] [Example 7]

[0063] 99.96 wt % of the polyethylene for artificial turf prepared in Example 1 and 0.04 wt % of CD-9 (compound additive) were mixed in a high-speed mixer at room temperature and pressure for 3 minutes, and then the temperature was controlled at 210° C. and granulated using a twin-screw extruder to obtain a special material for artificial turf. The physical properties of the special material for artificial turf were tested and analyzed, and the results are shown in Table 2.

[0064] [Example 8]

[0065] 99.965 wt % of the polyethylene for artificial turf prepared in Example 1 and 0.035 wt % of CD-9 (compound additive) were mixed in a high-speed mixer at room temperature and pressure for 3 minutes, and then the temperature was controlled at 210° C. and granulated using a twin-screw extruder to obtain a special material for artificial turf. The physical properties of the special material for artificial turf were tested and analyzed, and the results are shown in Table 2.

[0066] [Examples 9-11]

[0067] The method of Example 5 is followed, except that the polyethylene for artificial turf of Examples 2-4 is used respectively.

[0068] [Comparative Example 1]

[0069] The method of Example 1 and Example 5 is followed, except that the SLC-S catalyst is not used, that is:

[0070] In the presence of 300 ppm of triethylaluminum (co-catalyst), ethylene and 1-butene are subjected to a slurry polymerization reaction, and hydrogen as a molecular weight regulator is added simultaneously, wherein the hydrogen / ethylene molar ratio is 0.2, the 1-butene / ethylene molar ratio is 0.23, the reactor pressure is 2300 kPa, the reaction temperature is controlled at 86.5°C, and the ethylene partial pressure is 500 kPa, to obtain polyethylene for artificial grass.

[0071] 99.97 wt% of the prepared polyethylene for artificial grass and 0.03 wt% of CD-9 (compound additive) were mixed in a high-speed mixer at room temperature and pressure for 3 minutes, and then the temperature was controlled at 210° C. and granulated using a twin-screw extruder to obtain a special material for artificial grass. The physical properties of the special material for artificial grass were tested and analyzed, and the results are shown in Table 2.

[0072] Table 2

[0073] index Melt index (g / 10min) Yield stress (MPa) Yield strain (%) Example 5 2.51 12.8 17.0 Example 6 2.49 13.0 17.5 Example 7 2.50 13.1 18.4 Example 8 2.48 12.9 18.1 Example 9 2.52 12.6 19.1 Example 10 2.50 13.2 17.6 Embodiment 11 2.46 12.9 17.7 Comparative Example 1 2.51 11.2 16.6

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, as common knowledge in the field, other equivalent variations and improvements can also be made, which should also be regarded as the protection scope of the present invention.

Claims

1. An application of polyethylene in artificial turf, characterized in that: The polyethylene is obtained by slurry polymerization of ethylene and α-olefin in the presence of a Ziegler-Natta catalyst; the molar ratio of α-olefin to ethylene is 0.24-0.28:1; the catalyst is TiCl4 / MgCl2; the catalyst also includes an alkyl aluminum co-catalyst; the alkyl aluminum co-catalyst is at least one of triethyl aluminum, triethylbutyl aluminum and tri-tert-butyl aluminum; The α-olefin is selected from at least one of 1-butene, 1-hexene and 1-octene; The activity of the catalyst is 17000-23000 kg / kg; The catalyst is SLC-S; The polyethylene has a melt index of 1-5 g / 10 min at 2.16 kg and 190° C.

2. The use according to claim 1, characterized in that: The reaction also includes using H2 as a molecular weight regulator.

3. The use according to claim 1, characterized in that: The molecular weight distribution of the polyethylene is 3-6; and / or, The density of the polyethylene is 0.918-0.940 g / cm 3 .

4. The use according to claim 3, characterized in that: The polyethylene has a melt index of 1-4 g / 10 min at 2.16 kg and 190° C.; and / or, The molecular weight distribution of the polyethylene is 3.8-4.5; and / or, The density of the polyethylene is 0.918-0.930 g / cm 3 .

5. The use according to claim 2, characterized in that: The molar ratio of H2 to ethylene is 0.17-0.23:

1.

6. The use according to any one of claims 1 to 5, characterized in that: The reaction conditions include: temperature of 85-90°C and pressure of 1800-2800 kPa.

7. The use according to any one of claims 1 to 5, characterized in that: The application also includes compound additives.

8. The use according to claim 7, characterized in that: The compound additive comprises a hindered phenol antioxidant and a phosphite antioxidant.

9. The use according to claim 8, characterized in that: The compound additive includes antioxidant 1010 and antioxidant 168.

10. The use according to claim 7, characterized in that: The content of polyethylene is 99.96-99.98% by weight, and the content of compound additives is 0.02-0.04% by weight.

11. The use according to claim 7, characterized in that: The application comprises mixing polyethylene and compound additives and extruding the mixture.