A modified POE composition for photovoltaic film and its preparation method and application

Through the chemical graft modification and dual crosslinking system of the modified POE composition, the problem of slow crosslinking speed, insufficient adhesion and additive migration and precipitation of photovoltaic adhesive films is solved, which significantly improves the packaging efficiency and resistance of photovoltaic modules PID performance enables more efficient photovoltaic module manufacturing.

CN116023891BActive Publication Date: 2024-11-08ANHUI CHUZHO DEWEI NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310022562.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-08
Publication Date
2024-11-08
Estimated Expiration
2043-01-08

AI Technical Summary

Technical Problem

The existing photovoltaic adhesive films have problems such as slow crosslinking speed, insufficient adhesion, additive migration and precipitation and insufficient PID resistance, resulting in low packaging efficiency and short service life of photovoltaic modules.

Method used

Using a modified POE composition, silane monomer and glycidyl methacrylate GMA are grafted onto the POE macromolecular chain by chemical graft modification method, combining cross-linked sensitized polymers and cyclic unsaturated alkyl organics Silicon aid crosslinking agent forms a dual crosslinking system, which improves the crosslinking speed and adhesion of the adhesive film, and reduces the migration and precipitation of the additive.

Benefits of technology

It realizes rapid cross-linking, uniform adhesion, low VOCs emissions and strong PID resistance of photovoltaic adhesive films, and improves the yield and service life of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004043040860000041
    Figure BDA0004043040860000041
  • Figure BDA0004043040860000081
    Figure BDA0004043040860000081
  • Figure BDA0004043040860000082
    Figure BDA0004043040860000082
Patent Text Reader

Abstract

The present invention provides a modified POE composition for photovoltaic adhesive film, and a preparation method and application thereof. The raw material composition of the modified POE composition for photovoltaic adhesive film includes: 50-75% POE resin; 15-40% cross-linking sensitized polymer; 1-3% vinyl silane; 1-3% glycidyl methacrylate GMA; 0.1-0.5% initiator; 0.5% antioxidant; 0.5% light stabilizer; 1-5% liquid co-crosslinking agent. The present invention also provides a preparation method of the modified POE composition for photovoltaic adhesive film. The modified POE composition for photovoltaic adhesive film of the present invention can be used as a tackifier masterbatch and a co-crosslinking agent masterbatch in the formulation of photovoltaic adhesive film at the same time, and can also contribute to the crosslinking degree for the curing of the adhesive film through silane crosslinking, and cooperate with peroxide crosslinking to form a "double crosslinking system". The preparation method of the present invention is simple, has high production efficiency, and is easy to mass produce.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a POE composition, in particular to a modified POE composition for photovoltaic adhesive film and a preparation method and application thereof, belonging to the technical field of photovoltaic adhesive film. Background Art

[0002] With the proposal of the goal of "carbon peak and carbon neutrality", the market scale of new energy photovoltaic battery modules is expanding. As an important component of photovoltaic battery modules, photovoltaic film mainly serves as an adhesive layer to bond photovoltaic glass, photovoltaic cells and photovoltaic backplanes into photovoltaic modules. The key technical indicators of photovoltaic film are adhesion and cross-linking degree; the adhesion index includes the adhesion between the film and photovoltaic glass, photovoltaic backplane and photovoltaic cells; the cross-linking degree index represents the content of gel formed after the photovoltaic film is cross-linked and cured. The gel formed after the photovoltaic film is cross-linked and cured effectively improves the mechanical properties, heat resistance, creep resistance and weather resistance of the film. Photovoltaic film cross-linking and curing usually adopts thermal curing, which generally requires a high temperature of more than 140°C. The encapsulation time of photovoltaic film is generally as long as 20-30 minutes, and the molding cycle is relatively long. Therefore, the speed of cross-linking and curing of photovoltaic film directly affects the encapsulation efficiency of photovoltaic film. During the long-term operation of photovoltaic modules, potential induced degradation (PID) effect will occur. The PID effect is usually caused by the easy entry of water vapor into the edge of the photovoltaic module, and the high water absorption and water vapor permeability of EVA. After the EVA film is hydrolyzed, acetic acid will be generated. Acetic acid reacts with Na in the glass to generate a large number of free-moving Na ions, which will react with the silver grid lines on the surface of the battery cell, thereby corroding the battery grid lines, resulting in an increase in series resistance and module power attenuation. The attenuation degree can reach 50%. Therefore, anti-PID performance is also an important indicator for the quality of photovoltaic films. The general industry requires that the PID power attenuation of the back of the double-glass module battery after 192 hours is controlled within 5.0%. The current technical standards for photovoltaic films are GB / T 29848-2018 and T / CPIA0006-2017, which standardize the technical requirements and testing methods for EVA films and POE films.

[0003] At present, photovoltaic films are mainly EVA films and POE films. Among them, EVA films have the defects of low mechanical strength, high water vapor permeability, high water absorption, and poor weather resistance, which leads to poor anti-PID effect and short service life of double-glass modules after encapsulation. As a non-polar material, POE film has the advantages of low water vapor permeability and high volume resistivity, so it is more suitable for the encapsulation of double-glass modules. Compared with EVA film, it has a significant improvement in the anti-PID effect of modules. However, as a non-polar material, POE also has problems such as low adhesion to glass / backboard, slow cross-linking reaction rate, easy precipitation of functional additives and low light transmittance. Therefore, when pure POE is used in the module manufacturing process, problems such as reduced production efficiency and slippage during lamination will also occur, requiring the module factory to adjust the production process accordingly. In order to circumvent the shortcomings of EVA film and POE film, the current emerging technical route is EVA-POE-EVA (abbreviated as EPE) three-layer co-extrusion. EPE film has the characteristics of both anti-PID and good adhesion.

[0004] In view of the respective advantages and disadvantages of EVA and EPE, film companies developed three-layer co-extruded EPE films in 2018-2019. The three-layer co-extruded EPE film disclosed in CN108943936B has the advantages of anti-PID and low water vapor permeability in the middle layer POE, while the outer layer EVA solves the disadvantage of weak POE adhesion. The thickness ratio of the three layers of EPE film is usually 1:2:1. The biggest pain point of EPE is that the migration of additives brings about changes in film performance. EVA and POE have different polarities, and their absorption capacity for additives is very different: EVA is a polar material and has good compatibility with additives. Therefore, as time changes, the additives in the POE layer will continue to migrate to the EVA layer with strong polarity and strong absorption, causing changes in the internal structural properties of the film, and the bonding force between POE and EVA layers decreases. There is even a risk of the POE layer being squeezed out and delaminated during component lamination. Due to the characteristics of the migration of additives in the POE layer, the shelf life of EPE film is also shorter than that of EVA film and POE film.

[0005] In the existing technical route, free small molecule silane coupling agent is used as a tackifier. As the small molecule silane coupling agent migrates from the resin to the surface during film calendering, storage, and hot pressing, and then volatilizes and loses, the silane coupling agent in the system is lower than the original design amount in the terminal application, which may lead to insufficient and uneven adhesion between the film and the glass, backplane, and battery cell after the film is cured and encapsulated, directly leading to defects in photovoltaic modules, reduced yield of photovoltaic modules, and shortened service life of photovoltaic modules. CN111662655A discloses a POE photovoltaic film, which uses oily nanofillers, cage-type polysilsesquioxanes or cyclodextrin polymers as anti-precipitation agents to solve the problem of silane coupling agent precipitation, but at the same time brings about a decrease in the transmittance of the photovoltaic film.

[0006] In the existing technical route, the photovoltaic backplane is usually based on polyethylene terephthalate (PET for short), and a three-layer composite backplane is formed by bonding a fluorine-containing film on both sides of the PET substrate. The fluorine film of the photovoltaic backplane has excellent weather resistance, good mechanical properties and ductility; but the disadvantage is that the fluorine film is a fluorine polymer without polar groups, and it is difficult to combine with other hydrophilic groups, so that the adhesion between the photovoltaic film and the fluorine film layer of the backplane is relatively low, and the inner fluorine film surface needs to be treated by chemical or physical methods to improve its adhesion with the photovoltaic film. CN102850947B discloses a POE film with strong adhesion, which mainly improves the interfacial adhesion by adding a polar copolymer containing maleic anhydride, but there is no obvious improvement in the adhesion with the photovoltaic backplane.

[0007] In the existing technical route, since the POE film substrate itself is non-polar and has a saturated carbon chain structure, its cross-linking speed is slower than that of EVA. In order to increase the cross-linking degree and cross-linking speed of POE, the content of organic peroxide and co-cross-linking agent is usually increased, but this also brings the risk of increased bubbles. The residual peroxide in the component has also been confirmed to be the main factor causing "snail lines"; since the peroxide cross-linking of POE is a thermal cross-linking method, thermal curing is generally required for film encapsulation. Photovoltaic components generally need to be heated to a high temperature above 140°C, and the encapsulation time is generally as long as 20-30 minutes. The molding cycle is long, which seriously affects the efficiency of component encapsulation. WO2015096484A1 discloses a dual cross-linking technology of ultraviolet light cross-linking & peroxide cross-linking to improve the curing efficiency of the film, but the amount of auxiliary agent used is increased, and the film encapsulation process becomes a two-step process of ultraviolet light pre-irradiation and hot pressing curing, which makes the process complicated and lengthy.

[0008] Potential Induced Degradation (PID) is a common failure mode in the long-term operation of photovoltaic modules. The PID effect is usually caused by the easy entry of water vapor into the edge of the photovoltaic module, and the high water absorption and water vapor permeability of EVA. After the EVA film is hydrolyzed, acetic acid will be generated. Acetic acid reacts with Na in the glass to generate a large number of free-moving Na ions, which will react with the silver grid lines on the surface of the battery cell, thereby corroding the battery grid lines, resulting in an increase in series resistance and module power attenuation, with the degree of attenuation reaching 50%. Compared with EVA film, POE film has a significant improvement in the anti-PID effect of the module, but in the aging test and long-term use of the module, it was found that POE film also has the risk of PID failure on the back of the bifacial battery.

[0009] In the existing technical route, the photovoltaic film formula usually uses peroxides and co-crosslinking agents to achieve the crosslinking and curing of EVA or POE films. The conventional technical route uses resin particles and peroxides, co-crosslinking agents, coupling agents, antioxidants, light stabilizers, etc. to blend and then calender into films. Since the commonly used co-crosslinking agents are liquids, there is a problem of uneven mixing when mixing with the resin particles, which leads to uneven crosslinking of the photovoltaic film. In the existing technical route, polar small molecule additives such as peroxides, co-crosslinking agents, and silane coupling agents in the photovoltaic film formula are thermodynamically incompatible with POE, and are easily migrated and precipitated from the POE substrate during processing, and attached to the surface of the extruder screw, the inner surface of the die head, etc., and chemical reactions occur under long-term heating conditions, causing the film to burn. During the storage of the film, especially in low-temperature storage, the migration and precipitation of small molecule additives will also lead to problems such as insufficient crosslinking degree of the film, slow crosslinking speed, insufficient adhesion, and uneven adhesion, which will reduce the yield rate of photovoltaic modules and shorten their service life. At the same time, the migration, precipitation and volatilization of small molecule additives during film calendering, storage and hot pressing will produce volatile organic pollutants (VOCs), making the process less environmentally friendly.

[0010] Chemical grafting modification is a common modification technology for polyolefins. Peroxides are usually used to initiate the grafting of small molecule functional monomers containing double bonds onto polyolefin macromolecular chains, thereby achieving the anchoring of small molecule functional monomers on polyolefin macromolecular chains. The migration and precipitation of functional small molecule monomers in the main body of polyolefin materials and the concentration distribution gradient of functional small molecule monomers in polyolefin materials can be avoided. In addition, by grafting polar coupling agent functional monomers onto polyolefin macromolecular chains, polyolefin macromolecular coupling agents can be formed, which can improve the adhesion between polyolefins and polar interfaces (glass, battery cells and backplanes). Compared with the simple physical blending of polyolefins and small molecule coupling agents, polyolefin macromolecular coupling agents have more continuous and directly conductive adhesion, strong adhesion and uniform adhesion. Common polar coupling agent functional monomers include maleic anhydride MAH, glycidyl methacrylate GMA, methacrylic acid MA, unsaturated silane, etc. Among them, glycidyl methacrylate GMA contains epoxy groups, which can react with hydroxyl, amino, carboxyl or anhydride to form covalent bonds. Therefore, POE grafted with glycidyl methacrylate GMA has excellent reactivity with the terminal hydroxyl and terminal carboxyl groups of PET materials, so GMA-grafted POE has excellent adhesion to PET materials. Unsaturated silane grafting is also a common POE grafting modification method. The silane grafted to the POE main chain still retains the silicon-alkoxy group and can be hydrolyzed into silicon hydroxyl groups under natural conditions. The silicon hydroxyl groups can react with the hydroxyl groups on the glass surface and the cell surface to form chemically stable Si-O-Si bonds or Si-OC bonds. Therefore, unsaturated silane is the preferred auxiliary agent for improving the adhesion between polyolefins and glass surfaces. Most photovoltaic film formulations use silane coupling agents as tackifiers. In addition, after the silane grafted onto the POE main chain is hydrolyzed into silanol, a condensation reaction between silanol molecules will also occur, which can make the POE main chains grafted with silane cross-linked to form a gel network, which is called "silane cross-linking". Silane cross-linking, like peroxide cross-linking, is a preparation technology for thermosetting polyolefins. Silane is prone to hydrolysis when it encounters water molecules, which can effectively remove moisture from polyolefin materials and reduce the accumulation of water molecules in the film, so it also has the potential to resist PID.

[0011] Peroxide crosslinking of rubber and plastic materials usually uses C=C double bonds or tertiary carbon atom reaction sites to initiate the vulcanization or crosslinking of rubber and plastic materials; therefore, adding materials containing more double bonds or tertiary carbon atoms to polyolefin materials with saturated molecular chains can increase the crosslinking speed and degree of crosslinking of polyolefin materials. Such polymers containing more double bonds or tertiary carbon atoms can increase the vulcanization or crosslinking speed of other materials, namely "crosslinking sensitized polymers". Common crosslinking sensitized polymers include EPDM rubber, 1,2-polybutadiene rubber and hyperbranched polyethylene, etc.; and these three crosslinking sensitized polymers have excellent compatibility with polyolefin POE. For example, the hyperbranched polyethylene disclosed in CN109337156A can increase the speed and efficiency of free radical reactions such as grafting reactions and crosslinking reactions in polyolefin polymers. In addition, the cross-linking agent is also a common small molecule auxiliary agent that can improve the cross-linking speed and degree of cross-linking of polyolefin POE. Common cross-linking agents include trimethylolpropane trimethacrylate TMPTMA, triallyl isocyanurate TAIC, and triallyl cyanurate TAC. All three cross-linking agents are polar liquids with poor compatibility with polyolefin POE and are easy to migrate and precipitate from polyolefin materials. Therefore, the selection of cross-linking agents should fully consider their compatibility with POE materials. Cyclic unsaturated alkyl silicones are a new type of cross-linking agent. Commercial cyclic unsaturated alkyl silicones include trivinyltrimethylcyclotrisiloxane (V3), tetravinyltetramethylcyclotetrasiloxane (V4), and pentamethylpentavinylcyclopentasiloxane (V5). Since the molecular structure of cyclic unsaturated alkyl silicone cross-linking agents contains vinyl and methyl groups, this type of cross-linking agent has excellent compatibility with polyolefin POE and is not easy to migrate and precipitate from POE materials. Summary of the invention

[0012] In view of the shortcomings of the existing technical route, the purpose of the present invention is to provide a modified POE composition for photovoltaic film and a preparation method and application thereof.

[0013] In order to achieve the above-mentioned purpose, the present invention provides a modified POE composition for photovoltaic adhesive film. The modified POE composition for photovoltaic adhesive film aims to solve the problems of poor adhesion, slow crosslinking speed, migration and precipitation of auxiliary agents, uneven mixing of liquid auxiliary crosslinking agents, VOCs output and insufficient long-term PID resistance of conventional POE adhesive films.

[0014] The modified POE composition for photovoltaic adhesive film of the present invention, taking the sum of the raw material composition of the modified POE composition for photovoltaic adhesive film as 100%, the raw material composition of the modified POE composition for photovoltaic adhesive film is:

[0015]

[0016] In a specific embodiment of the present invention, the POE resin used is copolymerized by ethylene and α-octene, has a melt flow rate of 10 g / 10 min-40 g / 10 min, a melting point of ≤100° C., and a transmittance of ≥90%.

[0017] In a specific embodiment of the present invention, the cross-linked sensitized polymer used is one of EPDM rubber, 1,2-polybutadiene and hyperbranched polyethylene. Specifically, the mass percentage of ethylene norbornene ENB, the third monomer of EPDM rubber, is ≥3%; specifically, the molar proportion of 1,2-vinyl in the total vinyl content of 1,2-polybutadiene is ≥80%; specifically, the highly branched polyethylene is an ethylene homopolymer with a branched structure, and its branching degree is not less than 40 branches / 1000 carbon atoms; the melting point is ≤100°C.

[0018] In a specific embodiment of the present invention, the vinyl silane used is one or a combination of A-151 silane, A-171 silane, A-172 silane; specifically, the vinyl silane used is A-171 silane.

[0019] In a specific embodiment of the present invention, the initiator used is one or a combination of dicumyl peroxide, benzoyl peroxide, and di-tert-butyl peroxycumene. Specifically, the initiator is dicumyl peroxide;

[0020] In a specific embodiment of the present invention, the antioxidant used is one or a combination of antioxidant 1010, antioxidant 168 and antioxidant B215. Specifically, the antioxidant is antioxidant B215.

[0021] In a specific embodiment of the present invention, the light stabilizer used is one or a combination of light stabilizer UV-531, light stabilizer UV-P, light stabilizer 770, and light stabilizer 944. Specifically, the light stabilizer is a blend of light stabilizer UV-531 and light stabilizer 770 in a mass ratio of 1:1.

[0022] In a specific embodiment of the present invention, the liquid co-crosslinking agent used is a cyclic unsaturated alkyl organosilicon. Specifically, the cyclic unsaturated alkyl organosilicon used is one or a combination of trivinyltrimethylcyclotrisiloxane (V3), tetravinyltetramethylcyclotetrasiloxane (V4), pentamethylpentavinylcyclopentasiloxane (V5). Specifically, the liquid co-crosslinking agent used is tetravinyltetramethylcyclotetrasiloxane (V4).

[0023] The present invention also provides a method for preparing the modified POE composition for photovoltaic adhesive film, which comprises a two-step process of "co-blending grafting modification + impregnation absorption".

[0024] The first step is blending and grafting modification. Use a high-speed mixer to evenly mix POE resin, cross-linking sensitized polymer, vinyl silane, glycidyl methacrylate GMA, initiator, antioxidant and light stabilizer, and then feed the raw material mixture into a twin-screw extruder through a loss-in-weight feeder. Blending and grafting modification are carried out at a temperature of 180°C-200°C, and then granulation, dehydration and drying are performed to obtain POE grafted material.

[0025] The second step is immersion absorption. The POE grafted material and the liquid cross-linking agent are put into a rotary absorption chamber for mixing, and immersed under a heat preservation condition of 60°C until the POE grafted material fully absorbs the liquid cross-linking agent to obtain a modified POE composition for photovoltaic film.

[0026] The present invention also provides the application of the modified POE composition for photovoltaic film. The modified POE composition for photovoltaic film is directly used as a POE substrate in the photovoltaic film formula or as a tackifier masterbatch and a cross-linking agent masterbatch in the photovoltaic film formula. The modified POE composition for photovoltaic film is applied to photovoltaic film, and can contribute to the cross-linking degree of the film curing through silane cross-linking, and cooperate with the traditional peroxide cross-linking to form a "double cross-linking system" to improve the curing speed of the film.

[0027] In addition, after photovoltaic-grade POE or EVA resin is mixed with the modified POE composition for photovoltaic film of the present invention, POE or EVA photovoltaic film can be prepared; photovoltaic cells are encapsulated with the photovoltaic film containing the modified POE composition for photovoltaic film of the present invention, and the prepared photovoltaic film has the characteristics of fast cross-linking speed, strong adhesion to glass and backboard, uniform adhesion, less migration and precipitation of additives, low VOCs, etc.; the prepared photovoltaic module has the characteristics of strong anti-PID performance and high yield rate, etc.

[0028] The photovoltaic adhesive film prepared by using the modified POE composition for photovoltaic adhesive film of the present invention has the characteristics of strong adhesion to glass and backboard, uniform adhesion, fast cross-linking speed, less migration and precipitation of additives, strong anti-PID performance, etc.

[0029] Due to the application of the above technical solution, the technical principle and beneficial effects of the present invention are:

[0030] ① The modified POE composition for photovoltaic adhesive film of the present invention can be used as both a tackifier masterbatch and a cross-linking agent masterbatch in photovoltaic adhesive film;

[0031] ② The modified POE composition for photovoltaic adhesive film of the present invention grafts silane monomers onto POE macromolecular chains through a chemical grafting modification method to form a high molecular weight tackifier, which can effectively improve the adhesion between the adhesive film and the photovoltaic glass, and the adhesion is uniform, durable and stable. It solves the problems of migration and precipitation caused by the free small molecule silane tackifier used in the current conventional technical route, volatilization loss during the process, and VOCs output.

[0032] ③ The modified POE composition for photovoltaic adhesive film of the present invention grafts glycidyl methacrylate GMA monomer onto the POE macromolecular chain through a chemical grafting modification method to form a high molecular weight thickener. The epoxy group in GMA can undergo an epoxy ring-opening reaction with the terminal hydroxyl group and carboxyl group in the PET layer of the photovoltaic backplane to form a stable chemical bond, thereby greatly improving the adhesion between the photovoltaic adhesive film and the photovoltaic backplane.

[0033] ④ The modified POE composition for photovoltaic adhesive film of the present invention contains a cross-linking sensitized polymer, which can improve the cross-linking activity of the resin system; the prepared photovoltaic adhesive film has a faster cross-linking speed and a shorter hot pressing molding cycle, reduces the amount of small molecule auxiliary cross-linking agent used, and effectively avoids the migration and precipitation problem of small molecule auxiliary agents;

[0034] ⑤ The modified POE composition for photovoltaic film of the present invention grafts silane monomer onto POE resin by chemical grafting modification method. The modified POE composition can contribute to the crosslinking degree of film curing by silane crosslinking, and cooperate with traditional peroxide crosslinking to form a "double crosslinking system", which can increase the crosslinking speed of the film, shorten the curing cycle, and reduce the amount of peroxide and co-crosslinking agent in the photovoltaic film formula, thereby improving the problem of migration and precipitation of the auxiliary agent of the film, as well as the VOCs output and bubble defects caused by the thermal decomposition products of peroxide during the hot pressing packaging process;

[0035] ⑥ After the modified POE composition for photovoltaic film of the present invention is cross-linked and cured, the residual silane groups on the molecular chain of the modified POE composition can be used as a dehumidifier to continuously eliminate the moisture diffused into the film during the operation cycle of the photovoltaic module, thereby improving the anti-PID performance of the photovoltaic module;

[0036] ⑦ The modified POE composition for photovoltaic film of the present invention fully absorbs a quantitative amount of cyclic unsaturated alkyl silicone cross-linking agent through the "immersion absorption" process, and can be used as a solid cross-linking agent masterbatch in the photovoltaic film formula. It is not easy to migrate and precipitate, and is simple and convenient to use. The photovoltaic film formula does not need to add additional liquid cross-linking agent. The problem of uneven mixing of resin particles and liquid cross-linking agent is avoided, thereby ensuring the cross-linking uniformity of the photovoltaic film. DETAILED DESCRIPTION

[0037] The present invention is described in detail below through examples and comparative examples. The following examples are only used to further illustrate the present invention and do not limit the scope of protection of the present invention. Any non-essential improvements and adjustments made by technically skilled persons in any field based on the contents of the above invention should be covered within the scope of protection of the present invention.

[0038] The present invention is described using the following raw materials as examples:

[0039] POE resin uses ethylene-α-octene copolymer produced by Dow Chemical, with the brand name ENGAGE TM PV 8658.

[0040] The cross-linked sensitized polymer is one of ethylene propylene diene rubber, 1,2-polybutadiene or hyperbranched polyethylene.

[0041] The EPDM rubber adopts Dow Chemical NORDEL IP 5565, and the mass percentage of ethylidene norbornene ENB is 7.5%.

[0042] The 1,2-polybutadiene adopts the syndiotactic 1,2-polybutadiene manufactured by JSR Corporation, with the brand name JSR RB820, and the molar proportion of 1-2 vinyl in the total vinyl content is 92%.

[0043] Highly branched polyethylene HBPE is polymerized from ethylene using the catalyst and polymerization conditions disclosed in CN106589181B, and has a branching degree of 65 branches / 1000 carbon atoms; a weight average molecular weight of 150,000 Daltons, and a melting point of 75°C.

[0044] Vinyl silane uses vinyl trimethoxy silane manufactured by Jiangxi Chenguang New Materials Co., Ltd., with a brand name of A-171.

[0045] Glycidyl methacrylate GMA, made from Dow Chemical, has a purity of 99.58%.

[0046] The initiator used was dicumyl peroxide DCP manufactured by Jiangsu Daoming Chemical Co., Ltd.

[0047] As the antioxidant, AO B215 manufactured by BASF was used.

[0048] The light stabilizer is a mixture of UV 531 and light stabilizer UV 770 manufactured by BASF in a ratio of 1:1.

[0049] The liquid co-crosslinking agent is tetravinyltetramethylcyclotetrasiloxane manufactured by Hubei Silicon Yuan New Materials Co., Ltd., model V4.

[0050] The liquid auxiliary cross-linking agents used in the comparative example are trimethylolpropane trimethacrylate TMPTMA and triallyl isocyanurate TAIC.

[0051] Preparation of POE composition:

[0052] Preparation formula: refer to the raw material composition and ratio of the POE composition in Table 1 and Table 2.

[0053] Preparation process: The two-step process of "blending grafting modification + impregnation absorption" is adopted. The first step is blending grafting modification. The polyolefin elastomer ENGAGE TM PV 8658, cross-linking sensitizing polymer (NORDEL IP 5565, JSR RB820 or HBPE), vinyl silane A-171, glycidyl methacrylate GMA, initiator DCP, antioxidant AO B215 and light stabilizer UV531 / UV 770 are mixed evenly, and the raw material mixture is fed into a twin-screw extruder through a weight-loss feeding scale, and blended and grafted at a temperature of 180°C-200°C for modification, and then granulated, dehydrated and dried to obtain a POE grafted material; the second step is impregnation absorption, the POE grafted material and the liquid cross-linking agent are put into a rotary absorption bin for mixing, and impregnated at a temperature of 60°C until the POE grafted material fully absorbs the liquid cross-linking agent (V4, TMPTMA or TAIC). Finally, a modified POE composition for photovoltaic adhesive film disclosed in the present invention is obtained.

[0054] Table 1. Raw material composition and ratio of POE composition (I)

[0055]

[0056] Table 2. Raw material composition and ratio of POE composition (II)

[0057]

[0058] POE composition 9, maleic anhydride MAH is used to replace glycidyl methacrylate GMA in an equal amount, and other raw materials and proportions are the same as POE composition 1, and the preparation method remains unchanged;

[0059] POE composition 10 does not contain glycidyl methacrylate GMA, the amount of the formula is supplemented by A-171 silane, the other raw materials and proportions are the same as POE composition 1, and the preparation method remains unchanged;

[0060] POE composition 11, using γ-glycidyloxypropyltrimethoxysilane to replace A-171 silane in equal amounts; other raw materials and proportions are the same as POE composition 1, and the preparation method remains unchanged;

[0061] POE composition 12 does not contain A-171 silane, and the amount of the formula is supplemented by glycidyl methacrylate GMA. Other raw materials and proportions are the same as those of POE composition 1, and the preparation method remains unchanged;

[0062] POE composition 13, the formula does not contain liquid co-crosslinking agent V4, the amount of A-171 silane added is 3.7%wt, the other raw materials and proportions are the same as POE composition 1, and the preparation method remains unchanged;

[0063] POE composition 14, the formula raw materials and proportions are the same as those of POE composition 1; the preparation method is: the first step, blending and grafting modification, the raw materials except the liquid cross-linking agent are mixed in proportion and evenly fed into a twin-screw extruder through a loss-in-weight feeding scale, and blending and grafting modification are carried out at a temperature of 160°C-180°C, and then granulation, dehydration and drying are carried out to obtain a POE grafted material; the second step, the impregnation absorption process is the same as that of POE composition 1.

[0064] POE composition 15, the formula raw materials and proportions are the same as those of POE composition 1. The preparation method is: all raw materials are directly physically blended using a high-speed mixer.

[0065] Preparation of photovoltaic film:

[0066] The POE compositions 1 to 15 prepared above are directly used as POE substrates in photovoltaic film formulations or as tackifier masterbatches and crosslinking agent masterbatches in photovoltaic film formulations. POE or EVA photovoltaic films can be prepared by mixing the POE composition with photovoltaic-grade POE or EVA resin and peroxide crosslinking agent; photovoltaic cells are encapsulated using a photovoltaic film containing a modified POE composition for photovoltaic film prepared by the present invention;

[0067] In addition to the POE composition prepared by the present invention, the preparation of the photovoltaic film is described by taking the following materials as examples:

[0068] Photovoltaic grade POE resin, using POE PV8661 manufactured by Dow Chemical;

[0069] Photovoltaic grade EVA resin, using EVA EA28025 manufactured by LG Chemical;

[0070] Peroxide crosslinking agent, dicumyl peroxide DCP manufactured by Jiangsu Daoming Chemical Co., Ltd.;

[0071] The specific application description is given below through Examples 1 to 8 and Comparative Examples 1 to 14:

[0072] According to the photovoltaic film formula shown in Table 3, Table 4 and Table 5, the raw materials were put into a high-speed mixer for premixing for 6 minutes; added into a single-screw extruder for melt extrusion, the screw extruder temperature was set to 100°C, the screw speed was 100rpm, and finally through the extrusion, calendaring, cooling, cutting, and winding processes, the POE encapsulation film was obtained;

[0073] Table 3. Examples of preparing photovoltaic adhesive films, and their raw material compositions and ratios

[0074]

[0075] Table 4. Comparative examples of preparing photovoltaic adhesive films, and their raw material compositions and ratios (I)

[0076]

[0077]

[0078] Table 5. Comparative examples of preparing photovoltaic adhesive films, and their raw material composition and ratio (II)

[0079]

[0080] Wherein comparative example 13 and comparative example 14 are specifically described as follows:

[0081] Comparative Example 13: Directly preparing silane cross-linked POE using POE composition 13 and 0.05%wt dibutyltin dilaurate DBTDL

[0082] Photovoltaic adhesive film. The prepared photovoltaic adhesive film is not cured by peroxide crosslinking, but is completely cured by silane crosslinking. Comparative Example 14: The POE composition provided by the present invention is not used, and the traditional POE adhesive film formula, i.e., the formula of "POE resin + silane coupling agent + peroxide crosslinking agent + auxiliary crosslinking agent + antioxidant + light stabilizer" is used to mix the raw materials, and the prepared photovoltaic adhesive film is completely cured by peroxide crosslinking;

[0083] The POE films prepared in Examples 1 to 8 and Comparative Examples 1 to 14 were placed under natural conditions for 7 days and then subjected to performance tests according to the following test items and test methods.

[0084] Performance Test:

[0085] The specific test items and test methods are as follows:

[0086] Adhesion and adhesion uniformity test: The adhesion is characterized by testing the peel strength. The greater the peel strength, the greater the adhesion of the sample. Randomly sample 5 locations on the film sample, test the peel strength according to GB / T 2790-1995, calculate the average and variance of the 5 peel strength test values, and record the average as the peel strength of the sample. The variance represents the uniformity of the adhesion at different locations of the sample. The smaller the variance, the better the uniformity of the adhesion, and the larger the variance, the worse the uniformity of the adhesion.

[0087] Crosslinking speed test method: Take 45g of the test sample and place it in the torque rheometer. Mix it for 20 minutes at a heating temperature of 180°C and a rotor speed of 100rpm, while monitoring the torque change of the torque rheometer. The lowest measured torque value is designated as "ML" and is expressed in Newton meters (Nm). As the curing or crosslinking proceeds, the torque value increases and eventually reaches the maximum torque value. The maximum or highest measured torque value is designated as "MH" and is expressed in Newton meters (Nm). Under all other conditions being the same, the larger the MH torque value, the greater the degree of crosslinking. T 90 The cross-linking time is defined as the time required for the measured torque to reach (MH-ML)*90% of the torque value, expressed in minutes (min). 90 The shorter the crosslinking time, the faster the curing rate of the test sample. On the contrary, the longer the T90 crosslinking time, the slower the curing speed of the test sample.

[0088] Test method: GB / T 29848-2018 xylene extraction method

[0089] Cross-linking degree and cross-linking uniformity test method: Randomly sample 5 positions on the film sample and test the cross-linking degree according to the xylene extraction method of GB / T29848-2018. Calculate the average and variance of the 5 cross-linking degree test values, and record the average value as the cross-linking degree of the sample. The variance represents the uniformity of the cross-linking degree at different positions of the sample. The smaller the variance, the better the cross-linking uniformity, and the larger the variance, the worse the cross-linking uniformity.

[0090] Additive migration and precipitation test method (qualitative): 5 grams of the test sample containing the additive is placed in a separate unused polyethylene plastic ziplock bag, sealed and stored at room temperature for 15 days. After 15 days, the test sample is pressed together with the polyethylene plastic ziplock bag, and the oil stains left on the inner surface of the bag are observed under light. The oil stains indicate the degree of additive migration and precipitation in the test sample. The more oil stains on the inner surface of the bag, the more serious the additive precipitation of the test sample. According to the area of ​​the oil stains, the degree of additive precipitation can be recorded as none, very little, obvious, and very much to rank the precipitation amount.

[0091] Anti-PID performance test method: After the test sample is prepared into a photovoltaic film, it is hot-pressed and composited into a bifacial battery module. The test is carried out according to IECTS62804-1:2015. The test conditions are 85°C, 85% RH, and a negative 1500V constant DC voltage is applied. After 192 hours, the power attenuation percentage of the photovoltaic module before and after the PID test is determined.

[0092] Test results:

[0093] Table 6. Performance test results of examples and comparative examples

[0094]

[0095]

[0096] From the performance test data of the embodiments in Table 6, it can be seen that the photovoltaic adhesive film prepared in the embodiments has the characteristics of strong adhesion to glass and backboard, uniform adhesion, fast cross-linking speed, less migration and precipitation of additives, and strong anti-PID performance.

[0097] Compared with Example 1 and Example 2, the T 90 This indicates that the cross-linking speed of the photovoltaic film without or with little cross-linking sensitizer is slow, while the cross-linking speed of the photovoltaic film with sufficient cross-linking sensitizer is significantly accelerated.

[0098] Compared with Example 3, the peel strength of Example 3 with glass and backboard is significantly lower, indicating that A-171 silane and GMA grafting can simultaneously improve the adhesion between the photovoltaic film and the photovoltaic glass and the photovoltaic backboard.

[0099] Compared with Example 5, the auxiliary agent precipitation of Comparative Examples 4 and 5 is obvious, especially the precipitation of the auxiliary crosslinking agent leads to a larger variance of the crosslinking degree, that is, the crosslinking degree at different positions of the film is uneven. However, the auxiliary crosslinking agent V4 used in the present invention has good anti-precipitation property, the variance of the crosslinking degree of the examples is kept at a low level, and the crosslinking degree uniformity of the examples is good.

[0100] Compared with Example 1, the adhesion between Comparative Examples 6 and 7 and the photovoltaic backsheet is significantly poorer. The main variable is that Comparative Examples 6 and 7 did not use glycidyl methacrylate GMA for grafting. Therefore, it is proved that glycidyl methacrylate GMA grafted POE can greatly improve the adhesion between the film and the photovoltaic backsheet.

[0101] Compared with Example 1, the peel strength between the adhesive film prepared in Comparative Example 8 and the glass is significantly reduced and the variance is significantly larger, and the precipitation of the auxiliary agent is obvious, indicating that the free coupling agent γ-glycidyloxypropyltrimethoxysilane has poor precipitation resistance, which leads to uneven adhesion. This proves that Example 1 can effectively avoid the problems of decreased adhesion and uneven adhesion caused by the precipitation of the coupling agent by grafting POE with a silane coupling agent.

[0102] Compared with Example 1, the adhesion between the photovoltaic film prepared in Comparative Example 9 and the photovoltaic glass is poor. 90 The cross-linking time is long, and the PID power attenuation percentage is large. This shows that the problem of insufficient adhesion between the photovoltaic film and the photovoltaic glass can be effectively improved by grafting POE with a silane coupling agent in Example 1. In addition, the silane coupling agent grafted POE can contribute to the cross-linking degree through silane cross-linking, so the T90 cross-linking time is shortened. More surprisingly, the silane coupling agent grafted POE can also effectively improve the anti-PID performance of the photovoltaic film.

[0103] Compared with Example 1, Comparative Example 10 does not contain the auxiliary crosslinking agent V4, so the T90 crosslinking time of the photovoltaic adhesive film prepared in Comparative Example 10 is prolonged and the crosslinking degree is reduced, indicating that the auxiliary crosslinking agent V4 is an essential auxiliary component for the peroxide crosslinking of the photovoltaic adhesive film.

[0104] Compared with the preparation method of Example 1, since the preparation methods of Comparative Examples 11 and 12 are respectively a grafting temperature of 160-180°C and a simple physical blending, A-171 silane and glycidyl methacrylate GMA in the prepared POE compositions are in a free state, and thus the additive precipitates, which leads to the problem of decreased adhesion between the film and the glass and uneven adhesion.

[0105] Comparing Example 1, Comparative Example 13 and Comparative Example 14, it is found that the photovoltaic film T prepared by the "silane crosslinking + peroxide crosslinking" double crosslinking system adopted in Example 1 90 The cross-linking time is the shortest (the cross-linking speed is the fastest), the cross-linking degree is the highest, the cross-linking uniformity is the best, and there is no problem of additive precipitation.

[0106] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or modifications according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A modified POE composition for photovoltaic film, wherein the raw material composition of the modified POE composition for photovoltaic film is 100%, and the raw material composition of the modified POE composition for photovoltaic film is: POE resin 50%-75%; Cross-linked sensitized polymer 15%-40%; Vinyl silane 1%-3%; Glycidyl methacrylate GMA 1%-3%; Initiator 0.1%-0.5%; Antioxidant 0.5%; Light stabilizer 0.5%; Liquid cross-linking agent 1%-5%; The cross-linked sensitized polymer is ethylene propylene diene monomer rubber, 1,2-polybutadiene or hyperbranched polyethylene; The liquid auxiliary cross-linking agent is a cyclic unsaturated alkyl organosilicon, and the cyclic unsaturated alkyl organosilicon is one or a combination of trivinyltrimethylcyclotrisiloxane, tetravinyltetramethylcyclotetrasiloxane, pentamethylpentavinylcyclopentasiloxane; The preparation method of the modified POE composition for photovoltaic adhesive film comprises the following steps: Blending and grafting modification: POE resin, cross-linking sensitized polymer, vinyl silane, glycidyl methacrylate GMA, initiator, antioxidant and light stabilizer are uniformly mixed and then fed into a twin-screw extruder for blending and grafting modification to obtain a POE grafted material; The POE grafted material and the liquid cross-linking agent are put into a rotary absorption bin for mixing, and immersed under heat preservation conditions until the POE grafted material fully absorbs the liquid cross-linking agent and the surface is dry, thereby obtaining the modified POE composition for photovoltaic adhesive film.

2. The modified POE composition for photovoltaic adhesive film according to claim 1, wherein: The POE resin is copolymerized by ethylene and α-octene, has a melt flow rate of 10-40 g / 10 min, a melting point of ≤100° C., and a light transmittance of ≥90%.

3. The modified POE composition for photovoltaic adhesive film according to claim 1, wherein: The vinyl silane is one or a combination of A-151 silane, A-171 silane and A-172 silane.

4. The modified POE composition for photovoltaic adhesive film according to claim 1, wherein: The initiator is one or a combination of dicumyl peroxide, benzoyl peroxide, and di-tert-butyl peroxycumene.

5. The modified POE composition for photovoltaic adhesive film according to claim 1, wherein: The antioxidant is one or a combination of antioxidant 1010, antioxidant 168 and antioxidant B215.

6. The modified POE composition for photovoltaic adhesive film according to claim 1, wherein: The light stabilizer is one of light stabilizer UV-531, light stabilizer UV-P, light stabilizer 770, and light stabilizer 944, or a combination of several of them.

7. Use of the modified POE composition for photovoltaic adhesive film according to any one of claims 1 to 6, wherein the modified POE composition for photovoltaic adhesive film is simultaneously used for the viscosity-enhancing masterbatch and the cross-linking agent masterbatch in the photovoltaic adhesive film.