Lubricating grease and its preparation method and application
By saponifying the base oil, water and acid with the metal precursor and mixing it with the additive precursor, a grease containing metal soap thickening agent is prepared, which solves the insufficient performance of the existing space lubricant in special environments. Problem, excellent lubricity and stability are achieved.
Patent Information
- Application Number
- CN202111257806.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The existing space lubricants are insufficient in friction, wear and lubrication protection under special environments such as high temperature, high load, ultra-low temperature, ultra-high vacuum, strong radiation and strong corrosive media, and the adhesion, colloid stability and corrosion resistance are required. Further improvement.
A part of the base oil, water and acid are mixed with the metal precursor for saponification, and then mixed with the additive precursor to heat up and refine, then mixed with the residual base oil, and a zirconium precursor and/or titanium precursor as additives are used to form a containing content Grease for metal soap thickener.
It improves the oxidation resistance, adhesion, colloid stability and corrosion resistance of the grease, has low volatility and excellent lubricating properties, and is simple in preparation process and stable product quality.
Smart Images

Figure BDA0003324657590000071 
Figure BDA0003324657590000091 
Figure BDA0003324657590000121
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lubricating grease, and in particular to lubricating grease and a preparation method and application thereof. Background Art
[0002] Compared with conventional lubrication material technology, space lubrication material technology has its own particularity, which is mainly reflected in the fact that the application environment and motion conditions of space lubrication materials and technologies are very different from the atmospheric environment. Therefore, lubrication design is required according to the specific working conditions of each moving mechanism and moving parts.
[0003] Lubrication is usually achieved using liquid or solid lubricants. Among them, solid lubricating materials refer to solid materials that have good friction reduction and anti-wear properties. They can be specifically divided into three types: solid powder lubricating materials, solid lubricating films / coatings, and self-lubricating composite materials. The advantage of solid lubricants is that they can effectively solve the problems of friction, wear, and lubrication protection under special and harsh environmental conditions such as high temperature, high load, ultra-low temperature, ultra-high vacuum, strong radiation, and highly corrosive media. Its disadvantages are that the friction coefficient is large, it will produce debris and other contamination of the friction surface, the noise and vibration are large, and the self-repairing property is poor. As the working life of aerospace components becomes longer and longer, the speed becomes higher and higher, and the load becomes larger and larger, the demand for lubrication is also increasing. There is an urgent need to develop liquid lubricants with better lubricity and suitable for space environments. Liquid lubricants for space include space lubricating oils and greases. There are two main types of lubricants for space: synthetic oils and mineral oils. Commonly used synthetic oils include perfluoropolyether (PFPE), polyalphaolefin (PAO), polyalkylated cyclopentane (MAC), etc. Among them, MAC has both low saturated vapor pressure and excellent lubrication properties and is often used. In some working conditions that require grease lubrication, MAC is used as the base oil, and thickeners and additives are added to make grease. Greases based on MAC as the base oil have very low saturated vapor pressure and good lubrication properties, and can be widely used for the lubrication of moving parts in space. For example, US6218344B1 discloses a grease composition for satellites, which is composed of a base fluid with low volatility, a suitable thickener and about 0.1-9.9wt% of chlorine-free tris(phenoxyphenyl) phosphate, but its adhesion, colloid stability, corrosion resistance and other properties still need to be further improved. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a lubricating grease and a preparation method and application thereof.
[0005] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing grease on one hand, which comprises: mixing part of base oil, water, acid and metal precursor for saponification, mixing the saponification product with an additive precursor, heating and refining, and then mixing with the remaining base oil, wherein the additive precursor comprises a zirconium precursor and / or a titanium precursor, the zirconium precursor is selected from zirconium alkoxide and / or zirconium hydroxide, and the titanium precursor is selected from organic titanate and / or titanium hydroxide.
[0006] A second aspect of the present invention provides lubricating grease prepared by the above method.
[0007] The third aspect of the present invention provides a grease containing a metal soap thickener, additives and a base oil, wherein the additives include a first additive and / or a second additive, wherein the first additive is zirconium oxide and / or zirconium hydroxide, and the second additive is titanium oxide and / or titanium hydroxide.
[0008] A fourth aspect of the present invention provides the use of zirconium-containing substances and / or titanium-containing substances in improving the oxidation resistance of grease.
[0009] The lubricating grease of the present invention has low volatility (the additive used is a substance with low saturated vapor pressure) and excellent lubricity, and also has excellent adhesion, colloid stability (oxidation stability), corrosion resistance, etc. The lubricating grease of the present invention has a simple preparation process and stable product quality. DETAILED DESCRIPTION
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0011] The present invention provides a method for preparing grease, characterized in that the method comprises: mixing part of base oil, water, acid and metal precursor for saponification (reaction), mixing the saponification (reaction) product with an additive precursor, heating and refining, and then mixing with the remaining base oil, wherein the additive precursor comprises a zirconium precursor and / or a titanium precursor, the zirconium precursor is selected from zirconium alkoxide and / or zirconium hydroxide, and the titanium precursor is selected from organic titanate and / or titanium hydroxide.
[0012] In a preferred embodiment of the present invention, the additive precursor includes a zirconium precursor and a titanium precursor, and the amount ratio of the zirconium precursor calculated as Zr to the titanium precursor calculated as Ti is preferably 0.1-10:1 (such as 0.15, 0.18, 0.19, 0.5, 0.7, 1, 1.1, 2, 3, 4, 5, 5.1, 5.2, 5.5, 6, 8, 10 or any value between the above values), more preferably 0.2-5:1.
[0013] In the present invention, in order to further improve the stability and extreme pressure and anti-wear performance of the obtained grease, the method may further include: before mixing with the additive precursor, controlling the water content in the saponification product so that the ratio of the amount of water to the amount of the additive precursor calculated as a metal element is 1.5-3 (1.6, 1.8, 2, 2.2, 2.5, 2.8, 3 or any value between the above values). The water content in the saponification product can be monitored by conventional means. If the water content in the saponification product cannot meet the above preferred range, water can be added or heated to remove water to reach the content.
[0014] In the present invention, the amount of each raw material is not particularly limited. Relative to 100 parts by weight of base oil, the amount of water is preferably 1-20 parts by weight, and more preferably 5-15 parts by weight. The amount of metal precursor is sufficient to ensure that it reacts with acid to form a soap-based thickener. Relative to 100 parts by weight of base oil, the amount of metal precursor is preferably 0.01-20 parts by weight, and preferably 1-10 parts by weight (such as 1.4, 2, 2.5, 3, 3.5, 4.5, 5, 5.5, 6.5, 7.5, 8.5, 9.5 parts by weight or any value between the above values). Relative to 100 parts by weight of the base oil, the amount of the additive precursor calculated as the metal element can be 0.01-10 parts by weight, preferably 0.02-8 parts by weight (such as 0.02, 0.05, 0.08, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 2, 4, 6, 7 parts by weight or any value between the above values). Relative to 100 parts by weight of the base oil, the amount of the zirconium precursor calculated as Zr is preferably 0-10 parts by weight, more preferably 0.02-4 parts by weight (such as 0.05, 0.15, 0.2, 0.3, 0.4, 0.6, 1, 2, 3 parts by weight or any value between the above values). Relative to 100 parts by weight of the base oil, the amount of the titanium precursor calculated as Ti is preferably 0-10 parts by weight, more preferably 0.02-4 parts by weight (such as 0.03, 0.05, 0.1, 0.15, 0.2, 0.3, 0.4, 0.6, 1, 2, 3 parts by weight or any value between the above values). It can be understood by those skilled in the art that the sum of the amount of the partial base oil and the remaining base oil is the total amount of the base oil, and generally speaking, the weight ratio of the partial base oil to the remaining base oil is 2-10.
[0015] In the present invention, the zirconium alkoxide is a substance that can be decomposed into zirconium oxide (or zirconium hydroxide) at the reaction temperature. In a preferred embodiment of the present invention, the zirconium alkoxide is selected from zirconium alkoxides of C1-C20 (such as C2, C4, C6, C8, C10, C12, C14, C16 or C18), and is more preferably zirconium n-propoxide.
[0016] In the present invention, the organic titanate is a substance that can be decomposed into titanium oxide (or titanium hydroxide) at the reaction temperature. In a preferred embodiment of the present invention, the organic titanate is selected from C1-C20 (such as C2, C4, C6, C8, C10, C12, C14, C16 or C18) alkyl titanate, more preferably tetraisopropyl titanate.
[0017] In a preferred embodiment of the present invention, the kinematic viscosity of the base oil at 40°C is 1-600 mm 2 / s, kinematic viscosity at 100°C is 1-150mm 2 / s. The base oil is preferably polyalkyl cyclopentane.
[0018] In the present invention, the preparation method of polyalkyl cyclopentane may include:
[0019] After polyalkyl cyclopentadiene is diluted with C6-C12 alkane and mixed with an amorphous nickel catalyst, it is placed in a high-pressure reactor, hydrogen is introduced, and a hydrogenation reaction occurs under the conditions of a hydrogen pressure of 3-20 MPa and a temperature of 50°C-200°C, and the product polyalkyl cyclopentane is collected.
[0020] In the preparation method of polyalkyl cyclopentane, the polyalkyl cyclopentadiene is a mixture of cyclopentadiene containing 2-4 alkyl groups, wherein the weight contents of dialkyl cyclopentadiene, trialkyl cyclopentadiene and tetraalkyl cyclopentadiene are about 10-15%, 70-90% and 0-20%, respectively, wherein the alkyl group is a normal or isomeric alkyl group of C5-C24, such as n-decyl, isotridecyl, eicosyl, etc. The polyalkyl cyclopentadiene can be purchased from the market or prepared in accordance with the disclosed literature, for example, it can be prepared according to the following method: C5-C24 normal or isomeric alcohol, solid potassium hydroxide and dicyclopentadiene are mixed and added to a reaction flask equipped with a stirrer, a separatory funnel, a condenser, a water separator and a thermometer for heating. When no more water is produced in the water separator, the reaction is stopped. The reaction product is washed with water, dried and filtered to obtain polyalkyl cyclopentadiene.
[0021] In the preparation method of polyalkylcyclopentane, the alkane used as diluent is C6-C12 normal alkane, isoalkane or cycloalkane, preferably cyclohexane, n-heptane and decalin. The dilution ratio (dilution degree) of alkane to polyalkylcyclopentadiene is 1-50:100 (by mass), preferably 5-30:100.
[0022] In the method for preparing polyalkylcyclopentane, the weight amount of amorphous nickel is 0.1-10% of the weight of the polyalkylcyclopentadiene alkane diluent, preferably 0.8-3%.
[0023] In the preparation method of polyalkylcyclopentane, the reaction conditions are as follows: hydrogen pressure of 3-20 MPa, preferably 3-8 MPa, reaction temperature of 50-200° C., preferably 120-190° C., reaction time of 5-30 hours, preferably 15-20 hours. After the reaction is completed, the reactant is cooled, the material is taken out, filtered, and the diluent is removed to obtain the synthetic product polyalkylcyclopentane.
[0024] In the present invention, the base oil can be prepared by itself, for example, by referring to the method in CN1634815A.
[0025] In the present invention, those skilled in the art can select the acid and the metal precursor according to the type of thickener. For example, the acid can be a fatty acid of C12 or above, or a small molecule acid of C10 or below. The fatty acid can be a C12-C20 fatty acid, such as at least one of lauric acid, palmitic acid, stearic acid and 12-hydroxystearic acid, preferably 12-hydroxystearic acid and / or stearic acid. The small molecule acid can be an organic acid or an inorganic acid, preferably at least one of acetic acid, propionic acid, oxalic acid, adipic acid, azelaic acid, sebacic acid, phosphoric acid, benzoic acid and terephthalic acid.
[0026] In the present invention, the metal precursor can be selected from at least one of a Group IA metal precursor, a Group IIA metal precursor, a Group IIIA metal precursor, a Group IVA metal precursor, a Group IIB metal precursor, a Group IVB metal precursor and a Group VIIB metal precursor, preferably an alkali metal precursor and / or an alkaline earth metal precursor, more preferably at least one of lithium hydroxide, sodium hydroxide, calcium hydroxide and their hydrates.
[0027] In the present invention, the saponification conditions may include: a temperature of 80-120° C. and a time of 0.5-3 h.
[0028] In the present invention, the mixing conditions may include: a time of 20-30 minutes. There is no special requirement for the mixing temperature. According to a specific embodiment of the present invention, the method of the present invention does not need to additionally control the mixing temperature, that is, the mixing is carried out at a temperature close to the saponification temperature, and the additive precursor can also be directly added while hot after the saponification is completed.
[0029] In the present invention, the temperature-raising refining conditions may include: a temperature of 200-230° C. and a time of 3-20 min.
[0030] In the present invention, after mixing with the remaining base oil, the grease may be filtered, homogenized (grinded) or degassed in a conventional manner to obtain a finished grease product.
[0031] In a preferred embodiment of the present invention, in addition to the zirconium and titanium containing substances as described above, the method does not include using other forms of zirconium or titanium containing substances as raw materials for preparing grease.
[0032] In another preferred embodiment of the present invention, the method does not include the step of adding a grease antioxidant commonly used in the art (such as an aromatic amine antioxidant, which may be at least one of diphenylamine, phenyl-α-naphthylamine and diisooctyldiphenylamine). More preferably, the method consists only of the step of using the above ingredients.
[0033] The present invention also provides a lubricating grease prepared by the method as described above. In the method of the present invention, an additive precursor is used to synthesize the additive in situ, and the obtained lubricating grease has excellent antioxidant properties. On the one hand, the added zirconium alkoxide and organic titanate react with excess water in the system to generate zirconium hydroxide or zirconium dioxide and titanium hydroxide or titanium dioxide; on the other hand, the zirconium alkoxide and organic titanate may also react with the hydroxyl part of some long-chain alkyl carboxylates (thickeners) to generate a multifunctional additive having the following structure (the existence of the structure can be verified by infrared spectroscopy or determination of the hydroxyl value).
[0034]
[0035] In general, the addition of additive precursors may generate complex multifunctional additives, which give grease special properties, such as excellent colloidal stability, oxidation stability, extreme pressure and anti-wear properties, etc.
[0036] In addition, the present invention also provides a lubricating grease, characterized in that the lubricating grease contains a metal soap thickener, an additive and a base oil, wherein the additive includes a first additive and / or a second additive, wherein the first additive is zirconium oxide (zirconium dioxide) and / or zirconium hydroxide (zirconium hydroxide), and the second additive is titanium oxide (titanium dioxide) and / or titanium hydroxide (titanium hydroxide). As mentioned above, it can be understood that after the first additive and / or the second additive contact with the thickener, a structure shown in Formula I and / or Formula II may be generated, but the content of the first additive and / or the second additive described in the present invention is the total content of various forms of Zr and / or Ti.
[0037] According to a preferred embodiment of the present invention, the additive comprises a first additive and a second additive, and the molar ratio of the first additive calculated as Zr to the second additive calculated as Ti is preferably 0.1-10:1 (such as 0.15, 0.18, 0.19, 0.5, 0.7, 1, 1.1, 2, 3, 4, 5, 5.1, 5.2, 5.5, 6, 8, 10 or any value between the above values), more preferably 0.2-5:1.
[0038] According to the present invention, based on the total weight of the grease, the content of the thickener may be 5-70% by weight, preferably 7-50% by weight, and more preferably 8-20% by weight.
[0039] According to the present invention, based on the total weight of the grease, the content of the additive may be 0.1-25 wt %, preferably 0.5-20 wt %, and more preferably 0.8-15 wt %.
[0040] According to the present invention, based on the total weight of the grease, the content of the base oil may be 50-95% by weight, preferably 60-92% by weight, and more preferably 70-90% by weight.
[0041] According to the present invention, the content of the first additive calculated as Zr is preferably 0-10 parts by weight, more preferably 0.02-4 parts by weight (such as 0.05, 0.15, 0.2, 0.3, 0.4, 0.6, 1, 2, 3 parts by weight or any value between the above values) relative to 100 parts by weight of the base oil. The content of the second additive calculated as Ti is preferably 0-10 parts by weight, more preferably 0.02-4 parts by weight (such as 0.03, 0.05, 0.1, 0.15, 0.2, 0.3, 0.4, 0.6, 1, 2, 3 parts by weight or any value between the above values) relative to 100 parts by weight of the base oil.
[0042] According to the present invention, the base oil may be as described above, which will not be described in detail herein.
[0043] According to the present invention, the metal soap thickener can be various metal soap thickeners commonly used in the art (such as metal soaps such as lithium, sodium, calcium, aluminum, zinc, potassium, barium, lead, and manganese). According to a preferred embodiment of the present invention, the metal soap thickener is selected from at least one of lithium-based soaps, sodium-based soaps, and calcium-based soaps.
[0044] According to a preferred embodiment of the present invention, in addition to the zirconium and titanium containing substances as described above, the grease does not contain other forms of zirconium or titanium containing substances.
[0045] The present invention may also add common rust inhibitors, extreme pressure agents, anti-wear agents, oiliness agents, etc. as needed. According to another preferred embodiment of the present invention, the grease does not include common grease antioxidants in the art (such as aromatic amine antioxidants, which may be at least one of diphenylamine, phenyl-α-naphthylamine and diisooctyl diphenylamine), and more preferably, the grease consists only of the above ingredients.
[0046] The present invention also provides the use of zirconium-containing substances and / or titanium-containing substances in improving the oxidation resistance of grease. Wherein, the zirconium-containing substance is preferably selected from at least one of zirconium alkoxide, zirconium oxide and zirconium hydroxide. The titanium-containing substance is preferably selected from at least one of organic titanate, titanium oxide and titanium hydroxide. As mentioned above, the zirconium-containing substance may also include a substance having a structure shown in Formula I (generated by the reaction of zirconium alkoxide with the hydroxyl portion of a long-chain alkyl carboxylate (thickener)). The titanium-containing substance may also include a substance having a structure shown in Formula II (generated by the reaction of organic titanate with the hydroxyl portion of a long-chain alkyl carboxylate (thickener)).
[0047] In the above application, the molar ratio of the zirconium-containing substance in terms of Zr to the titanium-containing substance in terms of Ti can be 0.1-10:1 (e.g., 0.15, 0.18, 0.19, 0.5, 0.7, 1, 1.1, 2, 3, 4, 5, 5.1, 5.2, 5.5, 6, 8, 10 or any value therebetween), preferably 0.2-5:1. The specific types of the zirconium alkoxide and the organic titanate are as described above and will not be described in detail herein.
[0048] The present invention will be described in detail below through examples. In the following examples, the MAC base oil used was prepared according to the method described in CN1634815A, and typical parameters are shown in Table 1.
[0049] The method for monitoring its moisture content is GB / T 6283 "Determination of moisture content of chemical products - Karl Fischer method (general method)".
[0050] Multifunctional additive content = (lubricating grease weight - base oil feed amount - thickener theoretical production amount) / grease weight × 100%.
[0051] Table 1
[0052]
[0053] Example 1
[0054] Raw material components: 12-hydroxystearic acid (13 g); lithium hydroxide monohydrate (1.4 g); n-propanol solution of zirconium n-propoxide (70 wt %, 1.2 g); tetraisopropyl titanate (0.7 g); MAC (100 g).
[0055] 70g of MAC oil and 13g of 12-hydroxystearic acid were added to a reactor with a volume of 500mL, stirred, and heated to 85°C to form a homogeneous system. At this time, 1.4g of lithium hydroxide monohydrate and 5g of water were slowly added thereto, heated to 105°C for saponification for 2h, and then a mixture of 1.2g of n-propanol solution of zirconium n-propoxide and 0.7g of tetraisopropyl titanate was added to the above system while hot (the water content was monitored to be 0.18g), reacted for 30min, heated to 210°C, kept at a constant temperature for 5min, added 30g of MAC quenching oil, stirred and cooled, and then ground twice with a three-roll mill to obtain grease. The performance test results are shown in Table 2. According to the material feed amount, it can be calculated that the composition of the grease is: 88% by weight of base oil, 9% by weight of thickener, and 3% by weight of multifunctional additive.
[0056] Example 2
[0057] Raw material components: 12-hydroxystearic acid (11.5 g); azelaic acid (2 g); lithium hydroxide monohydrate (2.3 g); n-propanol solution of zirconium n-propoxide (70 weight %, 1 g); tetraisopropyl titanate (0.12 g); MAC (100 g).
[0058] In a reactor with a volume of 500mL, 90g of MAC oil, 11.5g of 12-hydroxystearic acid, and 2g of azelaic acid were added, stirred, and after heating to 90°C, 2.3g of lithium hydroxide monohydrate and 10g of water were slowly added thereto, and the temperature was raised to 95°C for saponification for 2h, and then a mixture of 1g of n-propanol zirconium solution and 0.12g of tetraisopropyl titanate was added to the above system while hot (the water content was monitored to be 0.09g), and the temperature was raised to 205°C after 20min of reaction, kept constant for 10min, 10g of MAC quenching oil was added, stirred and cooled, and then ground twice with a three-roll mill to obtain grease. The performance test results are shown in Table 2. According to the material feed amount, it can be calculated that the composition of the grease is: 87.7% by weight of base oil, 10.8% by weight of thickener, and 1.5% by weight of multifunctional additive.
[0059] Example 3
[0060] Raw material components: 12-hydroxystearic acid (5.85 g); acetic acid (7 g); calcium hydroxide (5.2 g); n-propanol solution of zirconium n-propoxide (70 weight %, 0.11 g); tetraisopropyl titanate (0.34 g); MAC (100 g).
[0061] 70 g of MAC and 5.85 g of 12-hydroxystearic acid were added to a reactor I with a volume of 500 mL, and the mixture was stirred and heated to 85° C. to form a homogeneous system.
[0062] In another container II, slowly add 5.2 g of calcium hydroxide into 8 g of water, stir evenly, then add 7 g of acetic acid, and react for 30 minutes before use.
[0063] The material in container II was slowly added to reactor I. After reacting for 1 hour, the temperature was raised to 110°C and drained and saponified for 1 hour. Then, while hot, a mixture of 0.11g of zirconium n-propoxide n-propanol solution and 0.34g of tetraisopropyl titanate was added to the above system (the water content was monitored to be 0.05g). After reacting for 30 minutes, the temperature was raised to 215°C and kept constant for 5 minutes. 30g of MAC quench oil was added, stirred and cooled, and then ground twice with a three-roll mill to obtain grease. The performance test results are shown in Table 2. According to the material feed amount, it can be calculated that the composition of the grease is: 86.4% by weight of base oil, 12.8% by weight of thickener, and 0.8% by weight of multifunctional additive.
[0064] Example 4
[0065] Raw material components: 12-hydroxystearic acid (6 g); stearic acid (8 g); benzoic acid (6 g); sodium hydroxide (3.2 g); n-propanol solution of zirconium n-propoxide (70 weight %, 1.9 g); tetraisopropyl titanate (1.7 g); MAC (100 g).
[0066] 70g of MAC lubricating base oil, 8g of stearic acid and 6g of benzoic acid were added to a 500mL atmospheric pressure reactor, heated to 90°C, 3.2g of sodium hydroxide and 15g of water were slowly added thereto, heated to 105°C for saponification for 2h, and then 6g of 12-hydroxystearic acid, 1.9g of n-propanol solution of zirconium n-propoxide and 1.7g of tetraisopropyl titanate were added to the above system while hot (the water content was monitored to be 0.36g), and the temperature was raised to 200°C after 30min of reaction, kept constant for 5min, 30g of MAC quench oil was added, stirred and cooled, and then ground twice with a three-roll mill to obtain grease. The performance test results are shown in Table 2. According to the material feed amount, it can be calculated that the composition of the grease is: 78.8% by weight of base oil, 15.8% by weight of thickener, and 5.4% by weight of multifunctional additive.
[0067] Example 5
[0068] Raw material components: 12-hydroxystearic acid (13 g); lithium hydroxide monohydrate (1.4 g); n-propanol solution of zirconium n-propoxide (70% by weight, 2.34 g); MAC (100 g).
[0069] The grease was prepared according to the method of Example 1, except that tetraisopropyl titanate was replaced with zirconium n-propoxide in an equal amount.
[0070] Example 6
[0071] Raw material components: 12-hydroxystearic acid (13 g); lithium hydroxide monohydrate (1.4 g); tetraisopropyl titanate (1.45 g); MAC (100 g).
[0072] The grease was prepared according to the method of Example 1, except that zirconium n-propoxide was replaced with an equal amount of tetraisopropyl titanate.
[0073] Comparative Example 1
[0074] Raw material performance components: 12-hydroxystearic acid (10 g); lithium hydroxide monohydrate (1.4 g); MAC (100 g).
[0075] 70g MAC oil and 10g 12-hydroxystearic acid were added to a reactor with a volume of 500mL, stirred, and heated to 80°C to form a homogeneous system. At this time, 1.4g lithium hydroxide monohydrate and 5g water were slowly added thereto, heated to 105°C for saponification for 2h, then heated to 210°C, kept at constant temperature for 10min, 30g MAC quench oil was added, stirred to cool, homogenized, filtered, degassed, and the grease was obtained from the reactor. The performance test results are shown in Table 2. According to the material feeding amount, it can be calculated that the composition of the grease is: 90.7% by weight of base oil and 9.3% by weight of thickener.
[0076] Comparative Example 2
[0077] A lubricating grease was prepared according to Comparative Example 1, except that poly-α-olefin (PAO10) was used instead of MAC as the base oil.
[0078] Table 2
[0079]
[0080]
[0081] Note: The larger the dropping point value, the better the high temperature performance of the grease; the smaller the 1 / 4 working cone penetration value, the stronger the thickening ability of the grease; the smaller the evaporation loss value, the longer the life of the grease; the smaller the steel mesh oil separation value, the better the colloid stability; the four-ball machine test P B Value and P D The larger the value and the smaller the d value, the stronger the extreme pressure and anti-wear performance; the smaller the pressure drop value, the better the oxidation stability.
[0082] It can be seen from the results in Table 2 that the lubricating grease of the present invention has low volatility and excellent lubricity, and also has excellent adhesion, colloid stability, corrosion resistance, etc. In addition, the preparation process of the lubricating grease of the present invention is simple.
[0083] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing grease, characterized in that: The method comprises: mixing part of base oil, water, acid and metal precursor for saponification, mixing the saponification product with additive precursor, heating and refining, and then mixing with the remaining base oil, wherein the acid is 12-hydroxystearic acid, the metal precursor is selected from at least one of IA group metal precursor, IIA group metal precursor, IIIA group metal precursor, IVA group metal precursor, IIB group metal precursor, IVB group metal precursor and VIIB group metal precursor, before the saponification product is mixed with the additive precursor, controlling the water content in the saponification product so that the amount ratio of water to the additive precursor calculated in terms of metal element is 1.5-3, the additive precursor comprises a zirconium precursor and a titanium precursor, the zirconium precursor is selected from zirconium alkoxide, the titanium precursor is selected from organic titanate, and the amount ratio of the zirconium precursor calculated in terms of Zr to the titanium precursor calculated in terms of Ti is 0.1-10:
1.
2. The method according to claim 1, wherein: The molar ratio of the zirconium precursor calculated as Zr to the titanium precursor calculated as Ti is 0.2-5:1; And / or, the amount of the additive precursor calculated as the metal element is 0.01-10 parts by weight relative to 100 parts by weight of the base oil.
3. The method according to claim 2, wherein: The amount of the additive precursor calculated as the metal element is 0.02-0.8 parts by weight relative to 100 parts by weight of the base oil.
4. The method according to claim 1, wherein: Relative to 100 parts by weight of base oil, the amount of water used is 1-20 parts by weight, the amount of metal precursor used is 0.01-20 parts by weight, the amount of zirconium precursor used in terms of Zr is greater than 0 and less than or equal to 10 parts by weight, and the amount of titanium precursor used in terms of Ti is greater than 0 and less than or equal to 10 parts by weight.
5. The method according to claim 1, wherein: The zirconium alkoxide is selected from C1-C20 zirconium alkoxides; And / or, the organic titanate is selected from C1-C20 alkyl titanates.
6. The method according to claim 1, wherein: The zirconium alkoxide is zirconium n-propoxide; And / or, the organic titanate is tetraisopropyl titanate.
7. The method according to claim 1, wherein: The kinematic viscosity of the base oil at 40°C is 1-600 mm 2 / s, kinematic viscosity at 100°C is 1-150mm 2 / s.
8. The method according to claim 1, wherein: The base oil is polyalkyl cyclopentane; And / or, the metal precursor is selected from at least one of lithium hydroxide, sodium hydroxide, calcium hydroxide and hydrates thereof.
9. The method according to claim 1, wherein: The saponification conditions include: temperature of 80-120°C and time of 0.5-3h; And / or, the temperature-raising refining conditions include: temperature of 200-230° C., time of 3-20 min.
10. Lubricating grease obtained by the method according to any one of claims 1 to 9.