A biofilm carrier material and preparation method thereof

Through the combination of modified biomass raw materials and activated biochar and other materials, high specific surface area, slow-release biofilm carrier materials are prepared, which solves the problems of poor microbial affinity and easy defilming of existing biofilm carrier materials, and achieves Stable sewage treatment and effective release of nutrients improve the treatment effect and material life.

CN116037080BActive Publication Date: 2024-10-11HENAN ACAD OF SCI POWER CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310069845.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-07
Publication Date
2024-10-11
Estimated Expiration
2043-02-07

AI Technical Summary

Technical Problem

When existing biofilm carrier materials are used to treat industrial wastewater and organic wastewater with low carbon and nitrogen content, they have poor microbial affinity, are prone to film removal, and are difficult to provide stable nutrients, resulting in poor treatment effects and difficulty in adding carbon sources and nutrients. control, may cause water pollution.

Method used

Using modified biomass raw materials, polyurethane micropowder, activated biochar and nutrients (such as potassium feldspar powder and apatite powder), through adjusting the pH value and thermoplastic molding, a slow-release carbon source with high specific surface area is prepared and biofilm carrier materials of nutritional elements to improve the adsorption capacity and growth environment of microorganisms.

Benefits of technology

It achieves rapid film formation and stable growth of microorganisms, avoids clogging of carrier materials, ensures sewage treatment effects, avoids secondary pollution of water bodies through a slow-release mechanism, and extends the service life of biofilm carrier materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116037080B_ABST
    Figure CN116037080B_ABST
Patent Text Reader

Abstract

The present invention provides a biofilm carrier material and a preparation method thereof, belonging to the technical field of biofilm carriers. The biofilm carrier material provided by the present invention comprises raw materials including solid phase components, adhesives and water; taking the mass of the solid phase components as 100%, the solid phase components include the following components: 10-60% modified biomass raw materials, 30-70% polyurethane micropowder, 5-15% activated biochar, 0.4-6% nutrients and 1-3% pore-forming agent; the mass ratio of the adhesive to the solid phase components is 1:(2-4). The results of the examples show that the specific gravity of the biofilm carrier material provided by the present invention is 0.45-0.60 g / cm 3 The porosity is 70-85%, the dissolved COD is 5-15 mg / g, and it has the function of slowly releasing nutrients such as carbon source, phosphorus, potassium, calcium and iron. It is suitable for biological treatment of various organic wastewaters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biofilm carriers, and in particular to a biofilm carrier material and a preparation method thereof. Background Art

[0002] The biofilm method is a method of treating wastewater by using microorganisms attached and grown on certain solid surfaces. It has the advantages of high treatment efficiency, resistance to shock loads, stable operation, low sludge production, and economic energy saving, and has been widely used in wastewater treatment. The biofilm is an ecosystem composed of high-density microorganisms and protozoa. The solid medium to which it is attached is called filter material or carrier. The core part is the material, roughness, and surface chemical properties of the biofilm carrier, which will directly affect the attachment of microorganisms and thus affect the wastewater treatment effect of the biofilm method. Most of the inorganic and organic biofilm carriers currently available on the market have poor biological affinity, long biofilm formation time, are hydrophobic, and have poor biofilm formation effects.

[0003] At present, the biofilm method mainly includes plastics and inorganic materials. The organic microbial film carrier made of plastic has high wear resistance and decomposition resistance, and the porosity and specific gravity can be controlled and adjusted, but its microbial affinity is poor, and it only provides a growth site for microbial growth, is easy to defilm, and cannot provide carbon sources and nutrients for microorganisms. Although the microbial film carrier made of inorganic materials (such as zeolite, activated carbon, and ceramsite) has a large specific surface area and strong physical adsorption, most of them have a large specific gravity and are difficult to provide growth nutrients for microorganisms. At the same time, it is easy to clog and requires regular backwashing.

[0004] Moreover, in actual application scenarios, for some special industrial wastewaters with relatively low carbon and nitrogen content and organic wastewaters that are difficult to treat, additional carbon sources such as methanol and glucose, and nutrients such as phosphorus and potassium need to be added to increase the concentration of microbial growth in the system and shorten the startup time of the biochemical treatment system. At the same time, it has the function of stabilizing the biochemical treatment system. However, this method has problems such as the difficulty in controlling the amount of carbon source and nutrient element addition, and is prone to cause water pollution.

[0005] Therefore, providing a biofilm carrier material that has strong adsorption capacity for microbial membranes, is not easily blocked, and can provide nutrients has become a technical problem that needs to be urgently solved in the field. Summary of the invention

[0006] The purpose of the present invention is to provide a biofilm carrier material and a preparation method thereof. The biofilm carrier material provided by the present invention has the characteristics of large specific surface area and strong adsorption capacity, so that microorganisms can be firmly adsorbed thereon and are not easy to remove from the film. At the same time, the pores of the biofilm carrier material are relatively large and are not easy to be blocked. The biofilm carrier material has the function of slowly releasing nutrients such as carbon source, phosphorus, potassium, calcium and iron, and is suitable for biological treatment of various types of organic wastewater.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a biofilm carrier material, the raw materials of which include solid phase components, adhesives and water;

[0009] Taking the weight of the solid phase component as 100%, the solid phase component comprises the following components: 10-60% of modified biomass raw material, 30-70% of polyurethane powder, 5-15% of activated biochar, 0.4-6% of nutrients and 1-3% of pore former; the nutrients comprise potassium feldspar powder and / or apatite powder;

[0010] The mass ratio of the binder to the solid phase component is 1:(2-4).

[0011] Preferably, the method for preparing the modified biomass raw material comprises: mixing hydrogen peroxide and the biomass raw material, adjusting the pH value to 10-12, and then performing a decolorization treatment to obtain the modified biomass raw material.

[0012] Preferably, the biomass raw material includes one or more of straw, plant vines, plant rhizomes, fruit shells and fermentation residues.

[0013] Preferably, the particle size of the biomass raw material is 60 to 300 meshes.

[0014] Preferably, the temperature of the decolorization treatment is 40-60° C., and the time of the decolorization treatment is 2-3 hours.

[0015] Preferably, the method for preparing the activated biochar comprises: activating the biochar in water vapor to obtain the activated biochar; the activation temperature is 400-600° C., and the activation time is 1-2 hours.

[0016] Preferably, the nutrient components are potassium feldspar powder and apatite powder.

[0017] Preferably, the pore-forming agent is sodium bicarbonate and / or ammonium bicarbonate.

[0018] Preferably, the adhesive comprises one or more of an aqueous polyurethane solution, a carboxymethyl cellulose solution, a starch solution and a guar gum solution.

[0019] The present invention provides a method for preparing the biofilm carrier material described in the above technical solution, comprising the following steps:

[0020] (1) mixing modified biomass raw materials, polyurethane powder, activated biochar, nutrients and pore-forming agents to obtain a solid phase component;

[0021] (2) mixing the solid phase component obtained in step (1) with a binder and water and stirring at a variable speed to obtain a paste;

[0022] (3) The paste obtained in step (2) is sequentially dried and thermoformed to obtain a biofilm carrier material.

[0023] The invention provides a biofilm carrier material, the raw materials of which include solid phase components, adhesives and water; based on the mass of the solid phase components as 100%, the solid phase components include the following components: 10-60% of modified biomass raw materials, 30-70% of polyurethane micropowder, 5-15% of activated biochar, 0.4-6% of nutrients and 1-3% of pore-forming agent; the nutrients include potassium feldspar powder and / or apatite powder; the mass ratio of the adhesive to the solid phase components is 1:(2-4). The present invention uses modified biomass raw materials as raw materials, which can slowly release carbon sources and nutrient elements on the one hand, and have strong microbial affinity on the other hand, so that microorganisms can grow and form biofilms quickly. By modifying the biomass raw materials, colored substances in the biomass raw materials can be removed, and the chromaticity impact of the color of the biomass raw materials themselves on water quality can be effectively reduced; the polyurethane micropowder has an adhesive effect in the thermoplastic molding process, and can promote the thermoplastic molding of the material in the process of preparing the biofilm carrier material; by adding biochar, the adsorption performance of the biofilm carrier material can be further improved, so that the microbial film is firmly fixed on the carrier material to avoid film removal; by activating the biochar, the ability of the biochar to capture and adsorb pollutants can be enhanced, and the adverse effects of impurities mixed in the biochar can be reduced; the nutrients can continuously release the nutrients required by the microorganisms, which can avoid secondary pollution of the water body caused by excessive nutrients, and can also improve the service life of the biofilm carrier material; the pore-forming agent can decompose and generate gas in the thermoplastic molding process, further improve the porosity of the biofilm carrier material, optimize the pore structure, and reduce blockage; the adhesive can improve the molding effect of the raw materials. The results of the examples show that the specific gravity of the biofilm carrier material provided by the present invention is 0.45-0.60 g / cm 3 The porosity is 70-85%, the dissolved COD is 5-15 mg / g, and the contents of dissolved nutrients are K: 0.4-0.8 mg / g, P: 0.18-0.4 mg / g, Ca: 0.1-0.3 mg / g, Fe: 0.1-0.3 mg / g. It has the function of slowly releasing carbon source, phosphorus, potassium, calcium and iron nutrients, and is suitable for biological treatment of various organic wastewaters. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a physical picture of the biofilm carrier material prepared in Example 1 of the present invention;

[0025] Figure 2 This is a physical picture of the biofilm carrier material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0026] The present invention provides a biofilm carrier material, the raw materials of which include solid phase components, adhesives and water;

[0027] Taking the weight of the solid phase component as 100%, the solid phase component comprises the following components: 10-60% of modified biomass raw material, 30-70% of polyurethane powder, 5-15% of activated biochar, 0.4-6% of nutrients and 1-3% of pore former; the nutrients comprise potassium feldspar powder and / or apatite powder;

[0028] The mass ratio of the binder to the solid phase component is 1:(2-4).

[0029] The present invention has no particular limitation on the specific sources of the raw materials in the biofilm carrier material, and commercially available products well known to those skilled in the art or self-prepared products may be used.

[0030] In the present invention, the solid phase component comprises 10-60% of the modified biomass raw material, preferably 20-50%, and more preferably 30-40%, based on the mass of the solid phase component being 100%. The present invention uses the modified biomass raw material as a raw material, which can slowly release carbon sources and nutrient elements on the one hand, and has strong microbial affinity on the other hand, so that the microorganisms can grow biofilm quickly.

[0031] In the present invention, the method for preparing the modified biomass raw material preferably comprises: mixing hydrogen peroxide and the biomass raw material, adjusting the pH value to 10-12, and then performing a decolorization treatment to obtain the modified biomass raw material.

[0032] In the present invention, the mass concentration of the hydrogen peroxide is preferably 3-6%, more preferably 4-5%. The present invention uses hydrogen peroxide to modify the biomass raw material, so that the colored substances in the biomass raw material can be oxidized and removed, which can effectively reduce the chromaticity effect of the color of the biomass raw material itself on the water quality.

[0033] In the present invention, the biomass raw material preferably includes one or more of straw, plant vines, plant rhizomes, fruit shells and fermentation residues. The present invention has no particular limitation on the specific source of the biomass raw material, and products well known to those skilled in the art can be used. The present invention uses the above substances as biomass raw materials, which can reduce production costs and is beneficial to environmental protection.

[0034] In the present invention, the particle size of the biomass raw material is preferably 60 to 300 meshes, more preferably 80 to 300 meshes, and further preferably 100 to 300 meshes. In the present invention, when the particle size of the biomass raw material does not meet the above conditions, the present invention preferably pulverizes the biomass raw material. The present invention does not have any special restrictions on the method of pulverization, as long as the particle size of the biomass raw material meets the requirements. The present invention can control the particle size of the biomass raw material to have a larger specific surface area, which is conducive to the biofilm formation of microorganisms.

[0035] In the present invention, the method of adjusting the pH value is preferably to add sodium hydroxide. The present invention has no particular limitation on the amount of sodium hydroxide used, as long as the pH value meets the requirements. The present invention controls the pH value of the solution, and under alkaline conditions, hydrogen peroxide can remove the color of the straw to a large extent. In addition, it can also break the dense structure of the biomass, expose the easily degradable cellulose, and slowly release polysaccharides or monosaccharides as a carbon source.

[0036] In the present invention, the temperature of the decolorization treatment is preferably 40 to 60° C., more preferably 50 to 60° C.; the time of the decolorization treatment is preferably 2 to 3 hours. The present invention can further improve the decolorization effect by controlling the parameters of the decolorization treatment.

[0037] In the present invention, based on the mass of the solid phase component being 100%, the solid phase component comprises 30-70% polyurethane micropowder, preferably 40-60%, and more preferably 50-60%. The present invention has no special limitation on the specific particle size of the polyurethane micropowder, and it can be selected according to the technical common sense of those skilled in the art. In the present invention, polyurethane micropowder is added as a raw material, and the polyurethane micropowder has an adhesive effect in the thermoplastic molding process, and can promote the thermoplastic molding of the material in the process of preparing the biofilm carrier material; by controlling the amount of polyurethane micropowder, the mechanical properties of the biofilm carrier material can be further improved.

[0038] In the present invention, based on the mass of the solid phase component being 100%, the solid phase component comprises 5-15%, preferably 9-15%, and more preferably 9-12% of activated biochar. In the present invention, the particle size of the activated biochar is preferably ≤100 mesh. By adding activated biochar, the adsorption performance of the biofilm carrier material can be further improved, so that the microbial film is firmly fixed on the carrier material to avoid film removal.

[0039] In the present invention, the preparation method of the activated biochar preferably comprises: activating the biochar in water vapor to obtain the activated biochar. The present invention can enhance the ability of the biochar to capture and adsorb pollutants and reduce the adverse effects of impurities contained in the biochar by activating the biochar.

[0040] In the present invention, the activation temperature is preferably 400-600°C, more preferably 450-550°C, and further preferably 500°C; the activation time is preferably 1-2h. The present invention can further improve the activation effect by controlling the activation time.

[0041] In the present invention, based on the mass of the solid phase component as 100%, the solid phase component includes 0.4-6% of the nutritional components. In the present invention, the nutritional components preferably include potassium feldspar powder and / or apatite powder, more preferably potassium feldspar powder and apatite powder. In the present invention, when the nutritional components are potassium feldspar powder and apatite powder, the amount of the potassium feldspar powder is preferably 0.2-3%, more preferably 0.5-2.5%, and further preferably 1-2%; the amount of the apatite powder is preferably 0.2-3%, more preferably 0.5-2.5%, and further preferably 1-2%. In the present invention, the particle size of the nutritional components is preferably ≤100 mesh. The present invention can achieve a sustained release effect by using the above-mentioned components as nutritional components and controlling their dosage, so that the nutritional components can be continuously released during the working process of the biofilm carrier material, which can not only avoid secondary pollution of water bodies caused by excessive nutritional components, but also improve the service life of the biofilm carrier material.

[0042] In the present invention, based on the mass of the solid phase component being 100%, the solid phase component includes 1 to 3% of the pore former, preferably 1 to 2%. In the present invention, the pore former is preferably sodium bicarbonate and / or ammonium bicarbonate, more preferably sodium bicarbonate or ammonium bicarbonate. In the present invention, the particle size of the pore former is preferably ≤ 100 mesh. In the present invention, by controlling the amount of the pore former, in the process of preparing the biofilm carrier material, the pore former can decompose and generate gas during the thermoplastic molding process, which can further improve the porosity of the biofilm carrier material, optimize the pore structure, and reduce clogging.

[0043] In the present invention, the adhesive preferably includes one or more of an aqueous polyurethane solution, a carboxymethyl cellulose solution, a starch solution and a guar gum solution, and more preferably an aqueous polyurethane solution, a carboxymethyl cellulose solution or a starch solution and a guar gum solution. In the present invention, the mass concentration of the aqueous polyurethane solution is preferably 20-40%, more preferably 25-35%, and further preferably 30%; the mass concentration of the carboxymethyl cellulose is preferably 1-2%; the mass concentration of the starch is preferably 5-20%, more preferably 10-15%; the mass concentration of the guar gum is preferably 0.5-3%, more preferably 1-2%. In the present invention, the adhesive mainly plays a shaping role on the raw material, so that it can maintain a certain shape before thermoplastic molding, thereby facilitating thermoplastic molding; by controlling the composition and concentration of the adhesive, its bonding effect can be further improved.

[0044] In the present invention, the mass ratio of the binder to the solid phase component is 1: (2-4), preferably 1: 3. The present invention can further improve the molding effect by controlling the amount of the binder and the solid phase component.

[0045] The present invention has no particular limitation on the amount of water used, and can be determined according to the technical common sense of those skilled in the art. In the present invention, the amount of water used is preferably such that the water content of the mixture of the solid phase component, the binder and the water is 30 to 60%.

[0046] The present invention uses modified biomass raw materials as raw materials, which can slowly release carbon sources and nutrient elements on the one hand, and have strong microbial affinity on the other hand, so that microorganisms can grow and form biofilms quickly. By modifying the biomass raw materials, colored substances in the biomass raw materials can be removed, and the chromaticity impact of the color of the biomass raw materials themselves on water quality can be effectively reduced; the polyurethane micropowder has an adhesive effect in the thermoplastic molding process, and can promote the thermoplastic molding of the material in the process of preparing the biofilm carrier material; by adding biochar, the adsorption performance of the biofilm carrier material can be further improved, so that the microbial film is firmly fixed on the carrier material to avoid film removal; by activating the biochar, the ability of the biochar to capture and adsorb pollutants can be enhanced, and the adverse effects of impurities mixed in the biochar can be reduced; the nutrients can continuously release the nutrients required by the microorganisms, which can avoid secondary pollution of the water body caused by excessive nutrients, and can also improve the service life of the biofilm carrier material; the pore-forming agent can decompose and generate gas in the thermoplastic molding process, further improve the porosity of the biofilm carrier material, optimize the pore structure, and reduce blockage; the adhesive can improve the molding effect of the raw materials.

[0047] The present invention provides a method for preparing the biofilm carrier material described in the above technical solution, comprising the following steps:

[0048] (1) mixing modified biomass raw materials, polyurethane powder, activated biochar, nutrients and pore-forming agents to obtain a solid phase component;

[0049] (2) mixing the solid phase component obtained in step (1) with a binder and water and stirring at a variable speed to obtain a paste;

[0050] (3) The paste obtained in step (2) is sequentially dried and thermoformed to obtain a biofilm carrier material.

[0051] The present invention mixes modified biomass raw materials, polyurethane powder, activated biochar, nutrients and pore-forming agents to obtain a solid phase component. In the present invention, the mixing method is preferably mechanical mixing. In the present invention, the particle size of the solid phase component is preferably ≤100 mesh. The present invention has no special restrictions on the specific operation of the mechanical mixing, as long as the components can be mixed evenly.

[0052] After obtaining the solid phase component, the present invention mixes the solid phase component with a binder and water and then stirs at a variable speed to obtain a paste.

[0053] In the present invention, the variable speed stirring method is preferably: first stirring and mixing at a low speed, and then stirring and foaming at a high speed. In the present invention, the rotation speed of the low speed stirring and mixing is preferably 300-500r / min; the time of the low speed stirring and mixing is preferably 8-12min; the rotation speed of the high speed stirring and foaming is preferably 800-1200r / min, more preferably 900-1100r / min, and further preferably 1000r / min; the time of the high speed stirring and foaming is preferably 2-5min, and more preferably 3-4min. The present invention mixes the solid phase component with the adhesive and water by means of variable speed stirring, and can make the components evenly mixed during the low speed stirring process, and then gradually introduces a large amount of air into the paste by high speed stirring, and makes the biofilm carrier material contain more bubbles by physical foaming, thereby increasing its porosity, optimizing the pore structure, and increasing its specific surface area, thereby increasing the adsorption rate of the microbial film on the biofilm carrier material, and avoiding film removal.

[0054] After the mixing is completed, the present invention preferably puts the mixed product into a molding die to obtain a paste. The present invention has no special limitation on the shape and size of the molding die, which can be determined according to the structure and size of the biofilm carrier material.

[0055] In the present invention, the water content of the paste is preferably 30 to 60%, more preferably 35 to 55%, and further preferably 40 to 50%.

[0056] After obtaining the paste, the present invention sequentially dries and thermoforms the paste to obtain the biofilm carrier material.

[0057] In the present invention, the drying temperature is preferably 30 to 60° C., more preferably 35 to 55° C., and further preferably 40 to 50° C.; the drying time is preferably 4 to 10 hours, more preferably 5 to 8 hours, and further preferably 6 to 7 hours. The present invention can remove most of the free water by controlling the drying parameters.

[0058] In the present invention, the temperature of the thermoplastic molding is preferably 130-170°C, more preferably 140-160°C, more preferably 150°C; the time of the thermoplastic molding is preferably 30-60 minutes, more preferably 40-50 minutes. The present invention controls the parameters of the thermoplastic molding. During the thermoplastic molding process, the pore-forming agent in the paste will be decomposed by heat to generate gas, forming a large number of bubbles in the paste, and the porosity of the biofilm carrier material is further increased by chemical foaming, so that it has a larger specific surface area, thereby increasing the adsorption rate of the biofilm carrier material to the microbial film and organic impurities in the wastewater, and can also avoid clogging.

[0059] In the present invention, the thermoplastic forming is preferably carried out in an oven. The present invention has no particular limitation on the type of the oven, and commercial products well known to those skilled in the art can be used.

[0060] After the thermoplastic molding is completed, the present invention preferably cools the thermoplastic molding product to obtain the biofilm carrier material. The present invention has no particular limitation on the cooling method, and furnace cooling or natural cooling can be used.

[0061] The present invention prepares the biofilm carrier material by combining high-speed stirring and thermoplastic forming. The high-speed stirring is physical foaming, and the thermoplastic forming is chemical foaming. The combination of physical foaming and chemical foaming greatly improves the specific surface area of ​​the biofilm carrier material and increases its porosity, so that the biofilm carrier material has a higher adsorption rate for microbial membranes and organic impurities in wastewater.

[0062] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0063] Example 1

[0064] A biofilm carrier material, the raw materials of which are composed of a solid phase component, a binder and water;

[0065] Taking the weight of the solid phase component as 100%, the solid phase component is composed of the following components: 12% of modified biomass raw material, 70% of polyurethane micropowder, 9% of activated biochar, 6% of nutrients and 3% of pore-forming agent;

[0066] The mass ratio of the binder to the solid phase component is 1:3;

[0067] The preparation method of the modified biomass raw material is as follows: after mixing hydrogen peroxide with a mass concentration of 5% and the biomass raw material, sodium hydroxide is added to adjust the pH value to 10, and then decolorization is performed to obtain the modified biomass raw material; the biomass raw material is straw, and the particle size of the biomass raw material is 60-300 meshes; the temperature of the decolorization treatment is 50° C., and the decolorization treatment time is 2 hours;

[0068] The preparation method of the activated biochar is as follows: activating the biochar in water vapor to obtain the activated biochar; the activation temperature is 500° C., and the activation time is 2 hours;

[0069] The nutrient components are feldspar powder and apatite powder, the amount of feldspar powder is 3%, and the amount of apatite powder is 3%;

[0070] The pore-forming agent is sodium bicarbonate;

[0071] The adhesive is a carboxymethyl cellulose solution, and the mass concentration of the carboxymethyl cellulose is 1.5%;

[0072] The preparation method of the biofilm carrier material consists of the following steps:

[0073] (1) mechanically mixing the modified biomass raw material, polyurethane powder, activated biochar, nutrients and pore-forming agent to obtain a solid phase component;

[0074] (2) mixing the solid phase component obtained in step (1) with a binder and water, stirring at a variable speed, and then loading into a molding mold to obtain a paste; the variable speed stirring method is: first stirring and mixing at a low speed, and then stirring and foaming at a high speed; the rotation speed of the low speed stirring and mixing is 400 r / min, and the time of the low speed stirring and mixing is 10 min; the rotation speed of the high speed stirring and foaming is 1200 r / min, and the time of the high speed stirring and foaming is 5 min; the water content of the paste is 50%;

[0075] (3) The paste obtained in step (2) is dried and thermoformed in sequence to obtain a biofilm carrier material; the drying temperature is 40° C. and the drying time is 8 hours; the thermoforming temperature is 170° C. and the thermoforming time is 30 minutes.

[0076] The actual picture of the biofilm carrier material prepared in Example 1 is as follows Figure 1 As shown. Figure 1 It can be seen that the biofilm carrier material prepared by the present invention has a loose structure and a large number of pore structures.

[0077] The structure of the biofilm carrier material prepared in Example 1 was tested, and the results showed that the specific gravity was 0.53 g / cm 3 , the porosity is 70%.

[0078] Example 2

[0079] Taking the weight of the solid phase component as 100%, the solid phase component is composed of the following components: 35% of modified biomass raw material, 47% of polyurethane micropowder, 15% of activated biochar, 2% of nutrients and 1% of pore-forming agent;

[0080] The mass ratio of the binder to the solid phase component is 1:2;

[0081] The nutrient components are feldspar powder and apatite powder, the amount of feldspar powder is 1%, and the amount of apatite powder is 1%;

[0082] The adhesive is an aqueous polyurethane solution, and the mass concentration of the aqueous polyurethane solution is 20%;

[0083] The temperature of the thermoplastic molding in step (3) is 150° C. and the time of the thermoplastic molding is 45 min;

[0084] Other conditions are the same as those in Example 1.

[0085] The actual picture of the biofilm carrier material prepared in Example 2 is as follows Figure 2 As shown. Figure 2 It can be seen that the biofilm carrier material prepared by the present invention has a loose structure and a large number of pore structures.

[0086] The structure of the biofilm carrier material prepared in Example 2 was tested, and the results showed that the specific gravity was 0.50 g / cm 3 , the porosity is 80%.

[0087] Example 3

[0088] Taking the weight of the solid phase component as 100%, the solid phase component is composed of the following components: 60% of modified biomass raw material, 30% of polyurethane micropowder, 8.6% of activated biochar, 0.4% of nutrients and 1% of pore-forming agent;

[0089] The mass ratio of the binder to the solid phase component is 1:4;

[0090] The nutrient components are feldspar powder and apatite powder, the amount of feldspar powder is 0.2%, and the amount of apatite powder is 0.2%;

[0091] The adhesive is a starch solution, and the mass concentration of starch in the starch solution is 20%;

[0092] The temperature of the thermoplastic molding in step (3) is 130° C. and the time of the thermoplastic molding is 60 min;

[0093] Other conditions are the same as those in Example 1.

[0094] The structure of the biofilm carrier material prepared in Example 3 was tested, and the results showed that the specific gravity was 0.46 g / cm 3 , the porosity is 85%.

[0095] Comparative Example 1

[0096] The slow-release carbon source particles developed by Shandong Haomiao Bioengineering Co., Ltd. use starch as the carbon source raw material, polyvinyl alcohol (PVA) as the carrier, and a-amylase as the additive. The solid carbon source material is encapsulated in a gel prepared from high molecular organic materials, and the composite slow-release carbon source is prepared by the freeze-cross-linking method using a cubic mold.

[0097] Comparative Example 2

[0098] The hydrophilic polyurethane sponge filler developed by DeChuang Environmental Protection has a specific surface area of ​​≥14000m 2 / m 3 , the porosity is 98%, which is a macroporous material.

[0099] Compared with Comparative Example 1, the biofilm carrier material provided by the present invention utilizes cellulose in biomass raw materials as the main carbon source material, supplemented with activated biochar as an adsorption material, and provides nutrients such as P, K, Ca, Fe, etc. required for microbial growth. Through low-temperature thermoplastic molding, not only the preparation method is simpler, but also the required preparation conditions are reduced. At the same time, the slow-release carbon source particles provided in Comparative Example 1 are mainly used to treat low-nitrogen water bodies with low carbon-nitrogen ratios to increase the carbon-nitrogen ratio in the water body, while the present invention treats nitrate nitrogen and organic impurities in wastewater, and the wastewater treated is more extensive.

[0100] Compared with Comparative Example 2, the biofilm carrier material provided by the present invention has stronger hydrophilicity and can provide nutrition and better growth space for the growth of microorganisms.

[0101] The nutrient slow-release effect of the biofilm carrier materials prepared in Examples 1 to 3 was tested. The test method was as follows: the biofilm carrier materials were placed in pure water for dissolution for 25 days, and the dissolved COD was 5 to 15 mg / g. The dissolved nutrient elements were K: 0.4 to 0.8 mg / g, P: 0.18 to 0.4 mg / g, Ca: 0.1 to 0.3 mg / g, and Fe: 0.1 to 0.3 mg / g. It can be seen that the biofilm carrier material provided by the present invention can release a variety of nutrient elements to help the reproduction of microorganisms.

[0102] The biofilm forming effect of the biofilm carrier materials prepared in Examples 1 to 3 was tested, and the test method was as follows: the biofilm carrier materials were placed in the prepared simulated wastewater, the water quality indicators of the wastewater were COD 600mg / L, nitrate nitrogen 188mg / L, and the denitrifying bacteria agent was used as the inoculum for testing. The test results were: biofilm formation began in 3 days, biofilm formation was completed in 7 to 10 days, and the microbial attachment amount was 30 to 40 mg / g in 15 days. It can be seen that the biofilm carrier material provided by the present invention can make microorganisms reproduce rapidly and form biofilms well.

[0103] The sewage treatment effect of the biofilm carrier material prepared in Example 1 was tested. The test method was as follows: the biofilm carrier material was placed in the prepared simulated wastewater, the water quality indicators of the wastewater were COD600mg / L, nitrate nitrogen 188mg / L, the experimental device was 5L, the height of the biofilm carrier material was 20cm, and after the biofilm was formed, water was continuously introduced, and the treatment was carried out at a temperature of 30°C and a pH of 6 for 6h. The test results were: 12mg / L nitrate nitrogen in the effluent, and the removal rate was 93.6%. It can be seen that the biofilm carrier material provided by the present invention has a good treatment effect on sewage.

[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A biofilm carrier material, the raw materials of which are composed of a solid phase component, a binder and water; Taking the weight of the solid phase component as 100%, the solid phase component comprises the following components: 10-60% of modified biomass raw material, 30-70% of polyurethane powder, 5-15% of activated biochar, 0.4-6% of nutrients and 1-3% of pore former; the nutrients comprise potassium feldspar powder and / or apatite powder; The mass ratio of the binder to the solid phase component is 1:(2-4); The preparation method of the modified biomass raw material comprises: mixing hydrogen peroxide and biomass raw material, adjusting the pH value to 10-12, and then performing a decolorization treatment to obtain the modified biomass raw material; The preparation method of the biofilm carrier material comprises the following steps: (1) mixing modified biomass raw materials, polyurethane powder, activated biochar, nutrients and pore-forming agents to obtain a solid phase component; (2) mixing the solid phase component obtained in step (1) with a binder and water and stirring at a variable speed to obtain a paste; (3) The paste obtained in step (2) is sequentially dried and thermoformed to obtain a biofilm carrier material.

2. The biofilm carrier material according to claim 1, It is characterized in that The biomass raw materials include one or more of straws, plant vines, plant rhizomes, fruit shells and fermentation residues.

3. The biofilm carrier material according to claim 1 or 2, It is characterized in that The particle size of the biomass raw material is 60 to 300 meshes.

4. The biofilm carrier material according to claim 1, It is characterized in that The temperature of the decolorization treatment is 40-60° C., and the time of the decolorization treatment is 2-3 hours.

5. The biofilm carrier material according to claim 1, It is characterized in that The preparation method of the activated biochar comprises: activating the biochar in water vapor to obtain the activated biochar; the activation temperature is 400-600° C., and the activation time is 1-2 hours.

6. The biofilm carrier material according to claim 1, It is characterized in that The nutrient components are potassium feldspar powder and apatite powder.

7. The biofilm carrier material according to claim 1, It is characterized in that The pore-forming agent is sodium bicarbonate and / or ammonium bicarbonate.

8. The biofilm carrier material according to claim 1, It is characterized in that The adhesive comprises one or more of an aqueous polyurethane solution, a carboxymethyl cellulose solution, a starch solution and a guar gum solution.

9. The method for preparing the biofilm carrier material according to any one of claims 1 to 8, The following steps are involved: (1) mixing modified biomass raw materials, polyurethane powder, activated biochar, nutrients and pore-forming agents to obtain a solid phase component; (2) mixing the solid phase component obtained in step (1) with a binder and water and stirring at a variable speed to obtain a paste; (3) The paste obtained in step (2) is sequentially dried and thermoformed to obtain a biofilm carrier material.