A method for expanding pores of an alumina carrier
Through the immersion and drying and calcining of ammonium chloride solution, the alumina carrier is re-energized, which solves the problem of damage to the pore structure during the molding process, improves the large pore content, is suitable for heavy oil hydrotreatment, and realizes the pore structure Effectively retain and improve.
Patent Information
- Application Number
- CN202111261206.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-28
AI Technical Summary
The pore structure of the existing alumina support is easily destroyed during the molding process, resulting in insufficient pore size and it is difficult to meet the demand for macropore content of heavy residue hydrotreatment catalysts.
The molded alumina carrier is immersed with ammonium chloride solution, and then dried and calcined to further amplify the pores to form a larger pore structure without destroying the original pores. This method is simple and easy to industrially produce.
The pore content of the alumina carrier is significantly improved by 10-30nm and 30-100nm, and the pore structure is well retained and is suitable for heavy oil hydrotreatment.
Smart Images

Figure CN116037086B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of inorganic material preparation, in particular to a pore expansion method for an alumina carrier. Background Art
[0002] With the increasing demand for crude oil worldwide and the increasing depletion of light crude oil resources, how to achieve efficient conversion of heavy crude oil has become an important trend in the development of oil refining technology. Most of the impurities such as metals, sulfur, nitrogen and residual carbon in crude oil are mainly enriched in the residual oil after atmospheric and vacuum distillation. These impurities must be removed in advance to prevent poisoning of hydrocracking catalysts. Residue oil raw materials have the characteristics of large molecular weight, complex structure and difficult diffusion. Therefore, the residue oil hydroprocessing catalyst is required to have a reasonable pore distribution to improve the mass transfer and diffusion of macromolecular reactants.
[0003] At present, the residual oil hydroprocessing catalyst generally uses Al2O3 as the carrier and Mo-Ni as the active component. The pore structure of the catalyst is generally determined by the alumina carrier, so the preparation of an alumina carrier with a larger pore structure is the key to increasing the macropore content of the residual oil hydroprocessing catalyst.
[0004] CN107913691A discloses an alumina carrier containing macropores and a preparation method thereof. The method uses styrene-butadiene rubber emulsion as a pore-enlarging agent. When preparing the carrier, styrene-butadiene rubber emulsion of a specified particle size is kneaded with pseudo-boehmite and sesbania powder, and then dried and calcined to obtain the alumina carrier containing macropores.
[0005] CN102861615A discloses a method for preparing a macroporous alumina carrier, which comprises mixing a certain amount of pseudo-boehmite, carbon black powder and an extrusion aid evenly, then adding an aqueous solution containing a peptizing agent and a chemical pore-enlarging agent, mixing the obtained materials evenly, extruding the materials into strips, and drying and calcining the formed materials to obtain the alumina carrier.
[0006] CN1120971A discloses a method for preparing an alumina carrier with a bimodal pore structure, wherein two or more pseudo-boehmite dry glue powders prepared by different raw material routes are uniformly mixed, and then peptized, molded, dried and calcined to obtain the alumina carrier.
[0007] Research has found that alumina carriers are generally made of pseudo-boehmite through kneading, drying and calcining. In order to increase the pore size of the final alumina carrier, people usually add physical pore expanders and / or chemical pore expanders when the alumina carrier is formed, or improve the pore structure of the alumina carrier by selecting specific pseudo-boehmite raw materials. The existing technology plays a certain role in increasing the pore size of the alumina carrier, but when the alumina carrier is formed, the kneading, extrusion and peptizing agent will have a certain destructive effect on the pores of the final carrier. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a method for expanding the pores of an alumina carrier. The method expands the pores of the formed alumina carrier again, and can further increase the macropore content of the carrier on the basis of the original pore structure of the alumina carrier. The method is simple in process and easy to industrialize. The prepared alumina carrier can be widely used in the field of heavy residue hydroprocessing.
[0009] The pore expansion method of an alumina carrier of the present invention comprises the following contents: impregnating a molded alumina carrier with an appropriate amount of ammonium chloride solution, drying and calcining the impregnated material to obtain an alumina carrier with expanded pores.
[0010] In the method of the present invention, the shaped alumina carrier can be of any shape, such as sphere, bar, special shape (three-leaf clover, four-leaf clover), etc. For example, the sphere has a particle size of generally 0.5-8.0 mm, and the bar, three-leaf clover, four-leaf clover and other shapes have a diameter of about 0.2-3.0 mm and a length of about 0.5-8.0 mm.
[0011] In the method of the present invention, there is no special requirement for the pore size of the shaped alumina carrier. Generally, the pore volume of pores with a pore size less than 10 nm accounts for 10%-45% of the total pore volume, the pore volume of pores with a pore size of 10-30 nm accounts for 30%-60% of the total pore volume, and the pore volume of pores with a pore size of 30-100 nm accounts for 1%-10% of the total pore volume. Preferably, the pore volume of pores with a pore size less than 10 nm accounts for 10%-35% of the total pore volume, the pore volume of pores with a pore size of 10-30 nm accounts for 45%-60% of the total pore volume, and the pore volume of pores with a pore size of 30-100 nm accounts for 2%-8% of the total pore volume.
[0012] In the method of the present invention, the alumina carrier can be prepared according to the existing method, generally, a proper amount of pseudo-boehmite powder, a peptizing agent, and an extrusion aid are kneaded, formed, dried, and calcined to obtain the alumina carrier; the pseudo-boehmite can be a pseudo-boehmite prepared by any method such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc.; the peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid and oxalic acid, and the amount of the peptizing agent added is 0.5wt%-3wt% of the weight of the alumina carrier; the extrusion aid is sesbania powder, and the amount of the extrusion aid added is 0.1wt%-0.5wt% of the weight of the alumina carrier; when the carrier is formed, a physical pore expander, such as carbon black powder, starch, methyl cellulose, etc., can be added as needed, and the amount of the physical pore expander added is 3%-10% of the weight of the alumina carrier; the drying temperature is 100-160°C, and the drying time is 4-10 hours; the calcining temperature is 450-600°C, and the calcining time is 4-6 hours; the calcining is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.
[0013] In the method of the present invention, the shaped alumina carrier may further contain a modifying element, such as one or more of phosphorus, boron, silicon, potassium, fluorine and the like, and the element content is 0.01%-5% by element. The modifying element may be added at any step in the preparation process of the alumina carrier, such as in the preparation process of pseudo-boehmite, in the kneading and shaping process of the alumina carrier, or in the alumina carrier precursor by impregnation.
[0014] In the method of the present invention, the mass percentage concentration of the ammonium chloride solution is 10%-35%, the amount of the solution used during impregnation is to completely immerse the alumina carrier, and the impregnation time is 0.5-1.5 hours. The impregnation is preferably performed twice, that is, the alumina carrier is first impregnated with an ammonium chloride solution with a mass percentage concentration of 10%-25%, and then dried and roasted; then the alumina carrier is impregnated again with an ammonium chloride solution with a mass percentage concentration of 20%-35%, and the impregnated material is dried and roasted to obtain the final alumina carrier.
[0015] In the method of the present invention, the drying temperature is 100-160°C, and the drying time is 4-10 hours; the roasting temperature is 550-700°C, and the roasting time is 4-6 hours; the roasting is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.
[0016] The macroporous alumina carrier prepared by the method of the present invention is used in the field of heavy oil hydrogenation. Compared with the prior art, the present invention has the following advantages: the method of the present invention re-expands the pores of the formed alumina carrier, which can increase the content of macropores on the basis of the original pores, and the pore structure formed after the pore expansion will not be destroyed by forming, extrusion or other effects, so that the formed macropores are well preserved, and the method is simple in process and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 1 and 2 are pore distribution diagrams of alumina carrier A1, alumina carrier S1 of Example 1, and alumina carrier S10 of Comparative Example 4. DETAILED DESCRIPTION
[0018] The technical scheme and technical effects of the present invention are further illustrated below in conjunction with embodiments, but are not limited to the following embodiments.
[0019] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 100nm were obtained according to the BJH model.
[0020] The technical scheme and technical effects of the present invention are further illustrated below in conjunction with embodiments, but are not limited to the following embodiments.
[0021] Forming alumina carrier preparation:
[0022] Weigh an appropriate amount of 100 g of pseudo-boehmite (prepared by the aluminum sulfate-sodium aluminate method), add 1.5 g of sesbania powder and 5 g of carbon black powder, mix the above materials evenly, then add an appropriate amount of aqueous solution containing 1.5 g of nitric acid and knead, extrude into clover-shaped strips with a particle diameter of about 1 mm and a length of 0.5-1 cm. Dry the molded material at 120°C for 4 hours, and then calcine at 600°C for 4 hours to obtain an alumina carrier A1. The properties of the carrier are shown in Table 1, and the carrier pore distribution diagram is shown in Table 1.
[0023] Weigh 100 g of a certain macroporous pseudo-boehmite, add 1.5 g of sesbania powder and 5 g of carbon black powder, mix the above materials evenly, then add a proper amount of aqueous solution containing 1.5 g of nitric acid and knead, extrude into cylindrical strips with a particle diameter of about 1.5 mm and a length of 0.5-1 cm. Dry the molded material at 120°C for 4 hours, and then calcine at 500°C for 5 hours to obtain alumina carrier A2. The properties of the carrier are shown in Table 1.
[0024] Example 1
[0025] Weigh 50 grams of the above-mentioned alumina carrier A1, first completely immerse the alumina carrier with an appropriate amount of 16.5wt% ammonium chloride solution for 0.5 hours, filter the impregnated material, dry it at 120°C for 6 hours, and then calcine it at 550°C for 4 hours. Then, completely immerse the alumina carrier precursor again with 27.5wt% ammonium chloride solution for 0.8 hours, filter the impregnated material, dry it at 120°C for 6 hours in an air atmosphere, and calcine it at 750°C for 4 hours to obtain the expanded alumina carrier S1. The properties of the carrier are shown in Table 1, and the carrier pore distribution diagram is shown in Table 1.
[0026] Example 2
[0027] Weigh 50 grams of the above-mentioned alumina carrier A1, first completely immerse the alumina carrier with an appropriate amount of 12.5wt% ammonium chloride solution for 1 hour, filter the impregnated material, dry it at 130°C for 5 hours, and then calcine it at 600°C for 4.5 hours. Then, completely immerse the alumina carrier again with 33.5wt% ammonium chloride solution for 0.5 hour, filter the impregnated material, dry it at 120°C for 6 hours in air atmosphere, and calcine it at 700°C for 4.5 hours to obtain the expanded alumina carrier S2. The properties of the carrier are shown in Table 1.
[0028] Example 3
[0029] Weigh 50 grams of the above-mentioned alumina carrier A2, first completely immerse the alumina carrier with an appropriate amount of 20.5wt% ammonium chloride solution for 0.8 hours, filter the impregnated material, dry it at 140°C for 4.5 hours, and then calcine it at 600°C for 4 hours. Then, completely immerse the alumina carrier again with 22.5wt% ammonium chloride solution for 1.2 hours, filter the impregnated material, dry it at 120°C for 8 hours in an air atmosphere, and calcine it at 650°C for 4 hours to obtain the expanded alumina carrier S3. The properties of the carrier are shown in Table 1.
[0030] Example 4
[0031] Weigh 50 grams of the above-mentioned alumina carrier A2, first completely immerse the alumina carrier with an appropriate amount of 23.5wt% ammonium chloride solution for 1.0 hour, filter the impregnated material, dry it at 135°C for 6 hours, and then calcine it at 650°C for 4 hours. Then, completely immerse the alumina carrier precursor again with 30.0wt% ammonium chloride solution for 0.5 hour, filter the impregnated material, dry it at 140°C for 4 hours, and calcine it at 700°C for 4 hours to obtain the expanded alumina carrier S4, the properties of which are shown in Table 1.
[0032] Example 5
[0033] Weigh 50 grams of the above-mentioned alumina carrier A1, and completely immerse the alumina carrier with an appropriate amount of 27.5wt% ammonium chloride solution for 1.2 hours. After filtering, the impregnated material is dried at 125°C for 6.5 hours, and then calcined at 700°C for 4.5 hours. The alumina carrier S5 after pore expansion is obtained, and the properties of the carrier are shown in Table 1.
[0034] Example 6
[0035] Weigh 50 grams of the above-mentioned alumina carrier A2, and completely immerse the alumina carrier with an appropriate amount of 26.5wt% ammonium chloride solution for 1.4 hours. After filtration, the impregnated material is dried at 130°C for 5.5 hours, and then calcined at 650°C for 5 hours. The alumina carrier S6 with expanded pores is obtained, and the properties of the carrier are shown in Table 1.
[0036] Comparative Example 1
[0037] The same method as Example 1 was used, except that the ammonium chloride was replaced with the same amount of ammonium oxalate to obtain an alumina carrier S5. The properties of the carrier are shown in Table 1.
[0038] Comparative Example 2
[0039] The same method as Example 3 was used, except that the ammonium chloride was replaced with the same amount of ammonium citrate to obtain an alumina carrier S6. The properties of the carrier are shown in Table 1.
[0040] Comparative Example 3
[0041] The same as Example 1, except that the ammonium chloride was replaced with distilled water, to obtain the alumina carrier S7. The properties of the carrier are shown in
[0042] Table 1.
[0043] Comparative Example 4
[0044] The same as Example 1, except that ammonium chloride was replaced with the same amount of ammonium bromide, to obtain an alumina carrier S8. The properties of the carrier are shown in Table 1, and the pore distribution diagram of the carrier is shown in Table 1.
[0045] Table 1 Alumina support properties
[0046]
[0047] As can be seen from Table 1, compared with the alumina carrier precursor, the alumina carrier prepared by the method of the present invention can significantly increase the pore content of 10-30nm and 30-100nm of the carrier after pore expansion. Compared with the comparative alumina carrier, the alumina carrier prepared by the method of the present invention has a higher pore content of 10-30nm and 30-100nm.
Claims
1. A method for expanding the pores of an alumina carrier, Features The method comprises the following steps: impregnating a molded alumina carrier with an appropriate amount of ammonium chloride solution, drying and calcining the impregnated material to obtain an alumina carrier with expanded pores; The impregnation is performed twice, i.e., firstly, the alumina carrier is completely impregnated with an ammonium chloride solution having a mass percentage concentration of 20.5%-25%, and then dried and calcined; then, the alumina carrier is completely impregnated again with an ammonium chloride solution having a mass percentage concentration of 20%-35%, and the impregnated material is dried and calcined to obtain the final alumina carrier.
2. The method according to claim 1, Features: The shaped alumina carrier is one or more of spherical, bar-shaped and special-shaped.
3. The method according to claim 1, Features: When the shaped alumina carrier is spherical, the particle size is 0.5-8.0 mm; when the shaped alumina carrier is strip-shaped, clover-shaped or four-leaf-shaped, the diameter is 0.2-3.0 mm and the length is 0.5-8.0 mm.
4. The method according to claim 1, Features: The pore size distribution of the shaped alumina carrier is as follows: the pore volume of pores with a pore size less than 10nm accounts for 10%-45% of the total pore volume, the pore volume of pores with a pore size of 10-30nm accounts for 30%-60% of the total pore volume, and the pore volume of pores with a pore size of 30-100nm accounts for 1%-10% of the total pore volume.
5. The method according to claim 1, Features: The pore size distribution of the shaped alumina carrier is as follows: the pore volume of pores with a pore size less than 10nm accounts for 10%-35% of the total pore volume, the pore volume of pores with a pore size of 10-30nm accounts for 45%-60% of the total pore volume, and the pore volume of pores with a pore size of 30-100nm accounts for 2%-8% of the total pore volume.
6. The method according to claim 1, Features: The drying temperature is 100-160° C., and the drying time is 4-10 hours.
7. The method according to claim 1, Features: The calcination temperature is 550-700°C, the calcination time is 4-6 hours, and the calcination is carried out in an air atmosphere.
8. Application of the macroporous alumina carrier prepared by the method according to claim 1 in the field of heavy oil hydrogenation.
Citation Information
Patent Citations
Preparation method of macroporous alumina carrier
CN102861615A
Macropore alumina carrier and preparation method thereof
CN107913691A
Prepn of alumina supporter
CN1120971A
Modification method of alumina carrier as well as preparation method and application of silver catalyst supported by alumina carrier
CN103357440A
High-activity heavy oil hydrogenation catalyst and preparation method thereof
CN112742407A