A low-hardness thermoplastic polyurethane elastomer that is easy to form and its preparation method and application
By adding acrylic copolymer high-density polyethylene, silicone acrylic microspheres and copolymerized wax to low-hardness thermoplastic polyurethane, the problems of long molding time and insufficient melt strength of low-hardness thermoplastic polyurethane elastomer are solved, and the molding time is shortened and the melt strength is shortened. The strength is improved, the material feels smooth, and the overall performance is significantly improved.
Patent Information
- Application Number
- CN202310059460.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-16
AI Technical Summary
Low-hardness thermoplastic polyurethane elastomers have problems in processing and melt strength, resulting in long molding times, high costs, and difficult-to-form materials.
Add acrylic copolymerized high-density polyethylene, silicone acrylic microsphere surface additives and copolymerized wax to thermoplastic polyurethane, and perform melt extrusion and granulation through a high-speed mixer and twin-screw extruder to optimize the material composition and processing conditions.
It significantly improves the melt strength and molding speed of the material, shortens the processing time, improves the compatibility and smoothness of the material, and has excellent overall performance.
Smart Images

Figure BDA0004061008640000051 
Figure BDA0004061008640000052 
Figure BDA0004061008640000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material modification, and relates to an easily moldable low-hardness thermoplastic polyurethane elastomer and a preparation method and application thereof. Background Art
[0002] The molecular chain segments of plastic polyurethane elastomer (TPU) are formed by the hard segment and the soft segment through covalent bonds, wherein the hard segment is mainly composed of diisocyanate, the soft segment is mainly composed of macromolecular diols, and the chain extender is a small molecule diol. According to the different soft segment structures, TPU can be divided into polyester TPU, polyether TPU, polycaprolactone TPU, polycarbonate TPU, etc., among which the commonly used TPUs are polyether type and polyester type. The soft segment forms a continuous phase to produce resilience, and the hard segment forms a hard segment area, which serves as a physical cross-linking point to produce excellent strength. When the hardness of TPU is low, the extruded wire is easy to bend, feels elastic, and is more popular with consumers. However, there are also certain problems. The melt strength of TPU itself is poor. Low-hardness TPU must have a high proportion of soft segments, which leads to slow crystallization of the material, difficulty in forming the material, too long cooling time, too narrow processing window, and easy degradation.
[0003] TPU products have excellent bearing capacity, impact resistance, shock absorption, wear resistance, and hand feel, and are deeply loved by consumers, but their processing and molding problems have always troubled manufacturers. For example, the Chinese patent application text (publication number: CN114031928A) discloses that at the polymerization end, the silica-supported organic tin is mainly concentrated in the hard segment region, and the tin atoms therein form coordination bonds with the carbamate groups in the hard segment region, which improves the extrusion molding problem of high-hardness TPU. The above patent is not applicable to the modified end and does not improve the extrusion molding problem of low-hardness TPU. The Chinese patent application text (publication number: CN109265972A) discloses the mixed modification of TPU with polystyrene, high-density polyethylene, vulcanizer, plasticizer, etc., which effectively improves the processing and molding problem of TPU, but more plasticizers are used to dissolve the plasticizers, and there is a risk of precipitation in the later stage, and TPU has poor compatibility with polystyrene and high-density polyethylene, which will affect the appearance of the product. The Chinese patent application text (publication number: CN107201023A) discloses that PTFE in the flame-retardant TPU system increases the melt strength and collapse resistance of TPU, but does not involve improving the processing and molding speed of TPU.
[0004] Therefore, this field is in urgent need of a material that improves the elastic processing and melt strength of low-hardness thermoplastic polyurethane to solve the problem of long processing time in the TPU wire field and save processing costs. Summary of the invention
[0005] The purpose of the present invention is to solve the above problems in the prior art and to provide an easily moldable low-hardness thermoplastic polyurethane elastomer, which effectively increases the melt strength of TPU by adding acrylic copolymer high-density polyethylene.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A thermoplastic polyurethane elastomer with low hardness that is easy to shape, wherein the raw materials of the thermoplastic polyurethane elastomer with low hardness that is easy to shape include, by weight:
[0008] Thermoplastic polyurethane elastomer: 75-90 parts,
[0009] Acrylic acid copolymer high-density polyethylene: 5-20 parts,
[0010] Surface additives: 1-5 parts,
[0011] Lubricant: 0.1~1 part,
[0012] Antioxidant: 0.1-1 part;
[0013] The acrylic acid content in the acrylic acid copolymer high-density polyethylene is greater than 6%.
[0014] Preferably, the thermoplastic polyurethane elastomer is polyether and / or polyester TPU with a hardness of 70A to 90A.
[0015] Further preferably, the thermoplastic polyurethane elastomer includes one or more of Meirui New Material Polyester TPU (E70, hardness 72A), Huafeng Polyester TPU (HF3385A, hardness 87A), Suzhou Austin Polyether TPU (580A, hardness 80A), and Wanhua Polyether TPU (WHT-8190, hardness 90A).
[0016] Preferably, the acrylic copolymer high-density polyethylene is SCONA TPPE 2400GAHD.
[0017] Preferably, the lubricant is copolymerized wax.
[0018] The carboxyl group in the copolymer wax is easier to combine with TPU than the ester group and has better compatibility.
[0019] Preferably, the surface additive is silicone acrylic microspheres, with a silicone content of 70% and a spherical shape.
[0020] Preferably, the antioxidant is one or more of 2,6-di-tert-butyl-4-methylphenol (antioxidant 264), pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1010), triphenyl phosphite (TPP), and tris(nonylphenyl) phosphite (TNPP).
[0021] The present invention also discloses a method for preparing a thermoplastic polyurethane elastomer with low hardness that is easy to form. The method comprises: weighing raw materials in proportion, putting them into a high-speed mixer and mixing them evenly, and then adding them into a feeding system of a twin-screw extruder to perform melt extrusion granulation to obtain a thermoplastic polyurethane elastomer with low hardness that is easy to form.
[0022] Preferably, the main engine speed is 300-500 r / min, and the processing temperature of each area is 170-200°C.
[0023] More preferably, the processing temperature of each region is 185-200°C.
[0024] The invention also discloses an application of a thermoplastic polyurethane elastomer with low hardness that is easy to form. The thermoplastic polyurethane elastomer with low hardness that is easy to form is extruded and formed. The wire diameter of the material is 2-5 mm, the skin thickness is 0.3-0.5 mm, and the extrusion speed is 50-60 m / min.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The low-hardness thermoplastic polyurethane elastomer that is easy to form is prepared by adding acrylic copolymer high-density polyethylene to thermoplastic polyurethane. Since HDPE has fast crystallization, excellent melt strength and fast forming, the melt strength of TPU is effectively increased and the forming processing time is shortened. Acrylic acid reacts with the amino acid ester in TPU to improve the compatibility of TPU and HDPE, thereby increasing the long side branches of TPU molecules and entangled with each other to increase the flow resistance of the chain segments, thereby further improving the melt strength of the TPU molecules.
[0027] 2. The easily moldable low-hardness thermoplastic polyurethane elastomer of the present invention uses silicone acrylic microspheres as surface additives. Since acrylic acid is more compatible with TPU and silicone resin gives the modified resin excellent smoothness, the material has an excellent feel.
[0028] 3. The copolymer wax in the easily moldable low-hardness thermoplastic polyurethane elastomer of the present invention helps the modified material flow and shape in the extruder, and has good compatibility with TPU, acrylic copolymer high-density polyethylene, and silicone acrylic microspheres, which helps the dispersion of the components.
[0029] 4. The easy-to-form low-hardness thermoplastic polyurethane elastomer of the present invention has a simple preparation process and strong operability.
[0030] 5. The easily moldable low-hardness thermoplastic polyurethane elastomer of the present invention has a melt strength index of less than 3 at 190° C. and 200° C., a short molding time, a fine surface, a smooth feel, and excellent comprehensive performance. DETAILED DESCRIPTION
[0031] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.
[0032] Test standard: tensile strength, elongation at break test standard: GB / T 528;
[0033] Melt flow rate (MFR) test standard: GB / T 3682.1-2018, test conditions: 190℃, 5kg;
[0034] Density test standard: GB / T1033;
[0035] Hardness test standard: GB / T 2411;
[0036] Melt Strength Index (MSI): tested on a melt indexer, MSI = outflow time of the first 10 cm / outflow time of the second 10 cm;
[0037] Molding and surface effects: The prepared TPU particles were extruded into flat wires in a single-screw flat wire machine and observed.
[0038] Embodiments 1 to 5
[0039] The raw materials were weighed according to the proportions described in Table 1, put into a high-speed mixer and mixed evenly, and then added to the feeding system of the twin-screw extruder for melt extrusion granulation; the main engine speed was 400 r / min, the processing temperature of each zone was 185-200°C, zone 1 was 185°C, zone 2 was 190°C, zone 3 was 200°C, the machine clamp was 200°C, and the die head was 190°C.
[0040] The specific performance is shown in Table 2.
[0041] Comparative Examples 1 to 7
[0042] The raw materials were weighed according to the proportions described in Table 1, put into a high-speed mixer and mixed evenly, and then added to the feeding system of the twin-screw extruder for melt extrusion granulation; the main engine speed was 400 r / min, the processing temperature of each zone was 185-200°C, zone 1 was 185°C, zone 2 was 190°C, zone 3 was 200°C, the machine clamp was 200°C, and the die head was 190°C.
[0043] The specific performance is shown in Table 2.
[0044] Table 1. Raw material addition data table
[0045]
[0046] Table 2. Performance data of the obtained thermoplastic polyurethane elastomer with low hardness and easy to form
[0047]
[0048]
[0049] Combining Table 1 and Table 2, it can be seen that Examples 1 to 5 use the raw materials of the present invention and control the raw material ratio, and the obtained easy-to-form low-hardness thermoplastic polyurethane elastomer has a melt strength index of less than 3 at 190°C and 200°C, a short molding time, a fine surface, a smooth feel, and excellent comprehensive performance. In Comparative Examples 1 and 2, acrylic copolymer low-density polyethylene is used to replace acrylic copolymer high-density polyethylene, and the crystallization is slow, resulting in the material melt strength index being too large and difficult to form; in Comparative Example 3, silicone masterbatch is used as a surface additive. Compared with silicone acrylic microspheres, the same amount of silicone masterbatch added in the whole system does not reach the effective content, and its effect is not reflected, resulting in an uneven feel of the product; in Comparative Example 4, the amount of silicone masterbatch added is further increased compared to Comparative Example 3. Although the feel is improved to a certain extent, it still does not reach the effective content, and due to the poor compatibility with TPU, the material compatibility is also poor. The surface is slightly rough and whitish; in Comparative Example 5, polyester wax is used instead of copolymer wax, and polyester wax is not easy to cover TPU, and the two are easy to separate, making the extruded material easy to stick to the flat wire head, the molding is unstable, the surface is slightly rough, and the feel is not smooth; in Comparative Example 6, the amount of TPU added is too little, and the amount of acrylic copolymer high-density polyethylene added is too much. The feel of the high-density polyethylene is not as good as that of TPU, resulting in a rough surface of the extruded material, the material is too hard, and the feel is not good; in Comparative Example 7, the amount of TPU added is too much, and the amount of acrylic copolymer high-density polyethylene added is too little. Due to the insufficient melt strength of TPU itself, it is not easy to mold, the molded product is easy to elongate, and the products are easy to stick to each other.
[0050] In summary, the easily moldable low-hardness thermoplastic polyurethane elastomer of the present invention is prepared by adding acrylic copolymer high-density polyethylene, silicone acrylic microsphere surface additive, copolymer wax and other raw materials into thermoplastic polyurethane, so that the melt strength index of the easily moldable low-hardness thermoplastic polyurethane elastomer under the conditions of 190° C. and 200° C. is less than 3, the molding time is short, the surface is fine, the hand feel is smooth, and the comprehensive performance is excellent.
[0051] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. An easily moldable low-hardness thermoplastic polyurethane elastomer, characterized in that: The raw materials of the easily moldable low-hardness thermoplastic polyurethane elastomer include, by weight: Thermoplastic polyurethane elastomer: 75~90 parts, Acrylic acid copolymer high-density polyethylene: 5~20 parts, Surface additives: silicone acrylic microspheres: 1~5 parts, Lubricant copolymer wax: 0.1~1 part, Antioxidant: 0.1~1 part; The acrylic acid content in the acrylic acid copolymer high-density polyethylene is greater than 6%; The silicone content of the surface additive is 70%; The copolymer wax is A-C400A or A-C540A.
2. The easily moldable low-hardness thermoplastic polyurethane elastomer according to claim 1, characterized in that: The thermoplastic polyurethane elastomer is polyether and / or polyester TPU, and has a hardness of 70A-90A.
3. The easily moldable low-hardness thermoplastic polyurethane elastomer according to claim 1 or 2, wherein the thermoplastic polyurethane elastomer comprises one or more of Meirui New Material Polyester TPU E70, Huafeng Polyester TPU HF3385A, Suzhou Austin Polyether TPU 580A, and Wanhua Polyether TPU WHT-8190.
4. The easily moldable low-hardness thermoplastic polyurethane elastomer according to claim 1, characterized in that: The acrylic copolymer high-density polyethylene is BYK SCONA TPPE 2400 GAHD.
5. The easily moldable low-hardness thermoplastic polyurethane elastomer according to claim 1, characterized in that: The antioxidant is one or more of 2,6-di-tert-butyl-4-methylphenol, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, triphenyl phosphite, and tris(nonylphenyl)phosphite.
6. The easily moldable low-hardness thermoplastic polyurethane elastomer according to claim 1, characterized in that: The melt strength index of the easily moldable low-hardness thermoplastic polyurethane elastomer under the conditions of 190° C. and 200° C. is less than 3.
7. A method for preparing the easily moldable low-hardness thermoplastic polyurethane elastomer as claimed in claim 1, characterized in that: The preparation method comprises: weighing raw materials in proportion, putting them into a high-speed mixer and mixing them evenly, then adding them into a feeding system of a twin-screw extruder, performing melt extrusion granulation, and obtaining an easily moldable low-hardness thermoplastic polyurethane elastomer.
8. The preparation method according to claim 7, characterized in that: The main machine speed is 300~500r / min, and the processing temperature of each area is 170~200℃.
9. An application of the easily moldable low-hardness thermoplastic polyurethane elastomer as claimed in claim 1, characterized in that: The low-hardness thermoplastic polyurethane elastomer which is easy to form is extruded and formed. The wire diameter of the low-hardness thermoplastic polyurethane elastomer which is easy to form is 2-5 mm, the skin thickness is 0.3-0.5 mm, and the extrusion speed is 50-60 m / min.
Citation Information
Patent Citations
Anti-dripping transparent flame-retardant TPU material and preparation method thereof
CN107201023A
Easy-to-process high-modulus matt TPU (Thermoplastic Polyurethane) elastomer and preparation method thereof
CN109265972A
High-hardness thermoplastic polyurethane elastomer composition suitable for extrusion and preparation method thereof
CN114031928A
Manufacturing method of TPU medical cable and medical cable
CN113861379A